Physical Properties | Original Value | Comments |
|
Density | 1.19 g/cc | Molded Foam; ASTM D 792 |
Density | 1.32 g/cc | ASTM D 792 |
Water Absorption | 0.14 % | 24 hours @ 73F; ASTM D 570 |
Water Absorption at Saturation | 0.3 % | Equilibrium, 73F; ASTM D 570 |
Linear Mold Shrinkage | 0.003 - 0.005 cm/cm | Flow, 0.250 inch; ASTM D 955 |
Mechanical Properties |
|
Tensile Strength @ Yield | 8500 psi | 0.250"; ASTM D 638 |
Elongation at Break | 3.6 % | 0.250"; ASTM D 638 |
Tensile Modulus | 620000 psi | 0.250"; ASTM D 638 |
Flexural Modulus | 745000 psi | 0.250"; ASTM D 790 |
Flexural Yield Strength | 15500 psi | 0.250"; ASTM D 790 |
Izod Impact, Unnotched | 8 ft-lb/in | 73F; ASTM D 4812 |
Falling Dart Impact | 32 ft-lb | 73F; GE Test |
Electrical Properties |
|
Volume Resistivity | 2.5e+017 ohm-cm | ASTM D 257 |
Surface Resistivity per Square | Min 1.1e+017 ohm | ASTM D 257 |
Dielectric Constant | 2.5 | 1 MHz; ASTM D 150 |
Dielectric Constant | 2.52 | 100 Hz; ASTM D 150 |
Dielectric Strength | 296 V/mil | in air, 250 mils; ASTM D 149 |
Dissipation Factor | 0.0008 | 100 Hz; ASTM D 150 |
Dissipation Factor | 0.0052 | 1 MHz; ASTM D 150 |
Comparative Tracking Index | 175 - 250 V | (+/- 0.125 inch); PLC Code 3; UL 746A |
Hot Wire Ignition, HWI | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
High Amp Arc Ignition, HAI | 30 - 60 arcs | Surface (+/- 0.125 inch); PLC Code 2; UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 80 - 150 mm/min | (+/- 0.125 inch); PLC Code 3; UL 746A |
Thermal Properties |
|
CTE, linear 68°F | 15 µin/in-°F | Flow, -40F to 200F; ASTM E 831 |
Specific Heat Capacity | 0.28 BTU/lb-°F | ASTM C 351 |
Deflection Temperature at 0.46 MPa (66 psi) | 290 °F | 0.250 inch, unannealed; ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 278 °F | 0.250 inch, unannealed; ASTM D 648 |
UL RTI, Electrical | 110 °C | UL 746B |
UL RTI, Mechanical with Impact | 110 °C | UL 746B |
UL RTI, Mechanical without Impact | 110 °C | UL 746B |
Flammability, UL94 | V-0 | 0.236 in. |
Flammability, UL94 | 7 | 0.236 in. |
Flammability Test | 0.85 | FOAM - Flame Class Minimum Density; g/cm3 |
Descriptive Properties |
|
Foam Weight Reduction | 10% | Mechanical Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Impact Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Thermal Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Physical Properties Reported Herein (0.250") |
Foam Weight Reduction | 20% | Electrical Properties Reported Herein (0.250") |
UL File Number, USA | E121562 | |