Physical PropertiesOriginal ValueComments
Density1.2 g/cc ASTM D 792
Water Absorption0.15 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation0.35 % Equilibrium, 73F; ASTM D 570
Water Absorption at Saturation0.58 % Equilibrium, 212F; ASTM D 570
Linear Mold Shrinkage0.005 - 0.007 cm/cm Flow, 0.125 inch; ASTM D 955
Melt Flow10.5 g/10 min 300C/1.2 kgf (O); ASTM D 1238

Mechanical Properties
Hardness, Rockwell M70 ASTM D 785
Hardness, Rockwell R118 ASTM D 785
Tensile Strength @ Break10000 psi Type I, 2.0 in/min; ASTM D 638
Tensile Strength @ Yield9000 psi Type I, 2.0 in/min; ASTM D 638
Elongation at Break130 % Type I, 2.0 in/min; ASTM D 638
Elongation at Yield7 % Type I, 2.0 in/min; ASTM D 638
Flexural Modulus340000 psi 0.05 in/min, 2" span; ASTM D 790
Flexural Yield Strength14000 psi 0.05 in/min, 2" span; ASTM D 790
Fatigue Strength1000 psi Fatigue Limit, 2.5 MM cycles; ASTM D 671
Izod Impact, Unnotched60 ft-lb/in 73F; ASTM D 4812
Gardner Impact @ 23°C565 in-lb Instrumented Impact Energy @ peak, 73F; ASTM D 3763
Tensile Impact Strength275 ft-lb/in² Type "S"; ASTM D 1822
Falling Dart Impact125 ft-lb 73F; ASTM D 3029
Taber Abrasion, mg/1000 Cycles10 CS-17, 1 kg; ASTM D 1044
Izod Impact, Notched15 ft-lb/in 73F; ASTM D 256

Electrical Properties
Volume ResistivityMin 1e+017 ohm-cm ASTM D 257
Dielectric Constant2.96 1 MHz; ASTM D 150
Dielectric Constant3.17 60 Hz; ASTM D 150
Dielectric Strength380 V/mil in air, 125 mils; ASTM D 149
Dissipation Factor0.0009 60 Hz; ASTM D 150
Dissipation Factor0.01 1 MHz; ASTM D 150
Comparative Tracking Index250 - 400 V (+/- 0.125 inch); PLC Code 2; UL 746A
Hot Wire Ignition, HWI30 - 60 sec (+/- 0.125 inch); PLC Code 2; UL 746A
High Amp Arc Ignition, HAI60 - 120 arcs Surface (+/- 0.125 inch); PLC Code 1; UL 746A
High Voltage Arc-Tracking Rate, HVTR25.4 - 80 mm/min (+/- 0.125 inch); PLC Code 2; UL 746A

Thermal Properties
CTE, linear 68°F38 µin/in-°F Flow, -40F to 200F; ASTM E 831
Specific Heat Capacity0.3 BTU/lb-°F ASTM C 351
Thermal Conductivity0.27 W/m-K ASTM C 177
Deflection Temperature at 0.46 MPa (66 psi)280 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)270 °F 0.250 inch, unannealed; ASTM D 648
Vicat Softening Point310 °F Rate B; ASTM D 1525
UL RTI, Electrical130 °C UL 746B
UL RTI, Mechanical with Impact130 °C UL 746B
UL RTI, Mechanical without Impact130 °C UL 746B
Flammability, UL94HB 0.028 in.

Optical Properties
Refractive Index1.586 ASTM D 542
Haze1 % 0.100 inch; ASTM D 1003
Transmission, Visible88 % 0.100 inch; ASTM D 1003

Descriptive Properties
Radiant Panel ListingUL tested 
UL File Number, USAE121562 
UV-light, water exposure/immersionF2 UL746C

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.