SABIC Innovative Plastics LEXAN HP1R Polycarbonate (Europe)


Subcategory: Polycarbonate; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesOriginal ValueComments
Density1.2 g/cc ASTM D 792
Density1.2 g/cc ISO 1183
Water Absorption0.1 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.15 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.35 % 23C; ISO 62
Water Absorption at Saturation0.58 % 100 C; ASTM D 570
Viscosity200000 cP Melt Viscosity; GE Test
Linear Mold Shrinkage0.005 - 0.007 cm/cm Flow; ASTM D 955
Melt Flow26 g/10 min cm3/10min; Melt Volume Rate, MVR at 300C/1.2 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M70 ISO 2039/2
Hardness, H358/3095 MPa ISO 2039/1
Tensile Strength, Ultimate50 MPa 50 mm/min; ISO 527
Tensile Strength, Yield63 MPa 50 mm/min; ISO 527
Elongation at Break70 % 50 mm/min; ISO 527
Elongation at Yield6 % 50 mm/min; ISO 527
Tensile Modulus2.35 GPa 1 mm/min; ISO 527
Flexural Modulus2.3 GPa 2 mm/min; ISO 178
Flexural Yield Strength90 MPa 2 mm/min; ISO 178
Izod Impact, Notched7 J/cm 23 C; ASTM D 256
Izod Impact, Notched (ISO)12 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)NB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NB 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp1.2 J/cm at -40 C; ASTM D 256
Izod Impact, Notched, Low Temp (ISO)10 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact, Notched, Low Temp1 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Notched1.2 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles10 CS-17, 1 kg; GE Test

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.7 50 Hz; IEC 60250
Dielectric Constant2.7 1 MHz; IEC 60250
Dielectric Strength15 kV/mm Short time, 3.2 mm; ASTM D 149
Dielectric Strength15 kV/mm Short time, 1.0 mm; IEC 60243-1
Dielectric Strength17 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength27 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength35 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.001 50 Hz; IEC 60250
Dissipation Factor0.01 1 MHz; IEC 60250
Arc Resistance114 sec Tungsten; ASTM D 495
Comparative Tracking Index125 V M; IEC 60112/3rd
Comparative Tracking Index225 V Natural; IEC 60112/3rd
Comparative Tracking Index250 V IEC 60112/3rd
Comparative Tracking Index250 V Stand. Black; IEC 60112/3rd
Comparative Tracking Index275 V Electr Grey; IEC 60112/3rd

Thermal Properties
CTE, linear 20°C70 µm/m-°C 23C-80C, flow; ISO 11359-2
Thermal Conductivity0.2 W/m-K ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)133 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)121 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)138 °C ASTM D 648
Vicat Softening Point139 °C B/50; ISO 306
Vicat Softening Point140 °C B/120; ISO 306
Vicat Softening Point145 °C A/50; ISO 306
Vicat Softening Point153 °C Rate B; ASTM D 1525
Flammability, UL94V-2 1.1 mm; UL 94 by GE
Flammability Test1.6 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
Oxygen Index25 % ISO 4589
Glow Wire Test850 °C Passes at 1 mm; IEC 60695-2-1

Optical Properties
Refractive Index1.586 ISO 489
HazeMax 0.8 % ASTM D 1003
Transmission, Visible88 - 90 % ASTM D 1003

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.