Physical PropertiesMetricEnglishComments
Density1.2 g/cc0.0434 lb/in³ ASTM D 792
Density1.2 g/cc0.0434 lb/in³ ISO 1183
Water Absorption0.1 %0.1 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.15 %0.15 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.35 %0.35 % 23C; ISO 62
Water Absorption at Saturation0.58 %0.58 % 100 C; ASTM D 570
Linear Mold Shrinkage0.005 - 0.007 cm/cm0.005 - 0.007 in/in Flow; ASTM D 955
Melt Flow6 g/10 min6 g/10 min cm3/10min; Melt Volume Rate, MVR at 300C/1.2 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M7070 ISO 2039/2
Hardness, H358/3095 MPa13800 psi ISO 2039/1
Tensile Strength, Ultimate70 MPa10200 psi 50 mm/min; ISO 527
Tensile Strength, Yield63 MPa9140 psi 50 mm/min; ISO 527
Elongation at Break120 %120 % 50 mm/min; ISO 527
Elongation at Yield6 %6 % 50 mm/min; ISO 527
Tensile Modulus2.35 GPa341 ksi 1 mm/min; ISO 527
Flexural Modulus2.3 GPa334 ksi 2 mm/min; ISO 178
Flexural Yield Strength90 MPa13100 psi 2 mm/min; ISO 178
Izod Impact, Notched7.5 J/cm14.1 ft-lb/in 23 C; ASTM D 256
Izod Impact, Notched (ISO)65 kJ/m²30.9 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)NBNB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NBNB 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)10 kJ/m²4.76 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact UnnotchedNBNB 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Unnotched Low TempNBNB at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched3.5 J/cm²16.7 ft-lb/in² 23 C; ISO 179/2C
Taber Abrasion, mg/1000 Cycles1010 CS-17, 1 kg; GE Test

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cmMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.72.7 50 Hz; IEC 60250
Dielectric Constant2.72.7 1 MHz; IEC 60250
Dielectric Strength15 kV/mm381 kV/in Short time, 3.2 mm; ASTM D 149
Dielectric Strength17 kV/mm432 kV/in in oil, 3.2 mm; IEC 60243-1
Dissipation Factor0.0010.001 50 Hz; IEC 60250
Dissipation Factor0.010.01 1 MHz; IEC 60250
Arc Resistance119 sec119 sec Tungsten; ASTM D 495
Hot Wire Ignition, HWI13 sec13 sec UL 746A
High Amp Arc Ignition, HAI70 arcs70 arcs on surface; UL 746A
High Voltage Arc-Tracking Rate, HVTR3.7 mm/min0.146 in/min UL 746A

Thermal Properties
CTE, linear 20°C70 µm/m-°C38.9 µin/in-°F 23C-80C, flow; ISO 11359-2
Thermal Conductivity0.2 W/m-K1.39 BTU-in/hr-ft²-°F ISO 8302
Hot Ball Pressure TestMax 140 °CMax 284 °F IEC 60335-1
Deflection Temperature at 0.46 MPa (66 psi)138 °C280 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)127 °C261 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)138 °C280 °F ASTM D 648
Vicat Softening Point144 °C291 °F B/50; ISO 306
Vicat Softening Point145 °C293 °F B/120; ISO 306
Vicat Softening Point153 °C307 °F Rate B; ASTM D 1525
Vicat Softening Point153 °C307 °F VST/A/120; DIN 53460
UL RTI, Electrical130 °C266 °F UL 746B
UL RTI, Mechanical with Impact125 °C257 °F UL 746B
UL RTI, Mechanical without Impact125 °C257 °F UL 746B
Flammability, UL94HBHB 0.75 mm
Oxygen Index25 %25 % ISO 4589
Glow Wire Test850 °C1560 °F Passes at 1 mm; IEC 60695-2-1

Optical Properties
Refractive Index1.5861.586 ISO 489
HazeMax 0.8 %Max 0.8 % ASTM D 1003
Transmission, Visible88 - 90 %88 - 90 % ASTM D 1003

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Hot Mandrel Test, 300 CPASSES CEE10/IIed
Water Absorption, 24 hours, mg10 DIN 53495

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.