SABIC Innovative Plastics LEXAN 925A Polycarbonate (Europe)


Subcategory: Polycarbonate; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesMetricEnglishComments
Density1.2 g/cc0.0434 lb/in³ ISO 1183
Moisture Absorption at Equilibrium0.15 %0.15 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.35 %0.35 % 23C; ISO 62
Linear Mold Shrinkage0.005 - 0.007 cm/cm0.005 - 0.007 in/in Flow; ASTM D 955
Melt Flow13 g/10 min13 g/10 min cm3/10min; Melt Volume Rate, MVR at 300C/1.2 kg; ISO 1133

Mechanical Properties
Hardness, H358/3095 MPa13800 psi ISO 2039/1
Tensile Strength, Ultimate60 MPa8700 psi 50 mm/min; ISO 527
Tensile Strength, Yield63 MPa9140 psi 50 mm/min; ISO 527
Elongation at Break85 %85 % 50 mm/min; ISO 527
Elongation at Yield6 %6 % 50 mm/min; ISO 527
Tensile Modulus2.35 GPa341 ksi 1 mm/min; ISO 527
Flexural Modulus2.3 GPa334 ksi 2 mm/min; ISO 178
Flexural Yield Strength90 MPa13100 psi 2 mm/min; ISO 178
Izod Impact, Notched (ISO)10 kJ/m²4.76 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)NBNB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NBNB 80*10*4 -30 C; ISO 180/ 1U
Charpy Impact UnnotchedNBNB 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Unnotched Low TempNBNB at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cmMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.72.7 50 Hz; IEC 60250
Dielectric Constant2.72.7 1 MHz; IEC 60250
Dielectric Strength17 kV/mm432 kV/in in oil, 3.2 mm; IEC 60243-1
Dissipation Factor0.0010.001 50 Hz; IEC 60250
Dissipation Factor0.010.01 1 MHz; IEC 60250

Thermal Properties
CTE, linear 20°C70 µm/m-°C38.9 µin/in-°F 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow70 µm/m-°C38.9 µin/in-°F 23C-80C; ISO 11359-2
Thermal Conductivity0.2 W/m-K1.39 BTU-in/hr-ft²-°F ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)135 °C275 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)124 °C255 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point141 °C286 °F B/50; ISO 306
Vicat Softening Point142 °C288 °F B/120; ISO 306
UL RTI, Electrical130 °C266 °F UL 746B
UL RTI, Mechanical with Impact120 °C248 °F UL 746B
UL RTI, Mechanical without Impact125 °C257 °F UL 746B
Flammability, UL94V-2V-2 1.5 mm
Flammability, UL94V-0V-0 3 mm
Oxygen Index35 %35 % ISO 4589
Glow Wire Test850 °C1560 °F Passes at 1 mm; IEC 60695-2-1
Glow Wire Test960 °C1760 °F Passes at 1.6 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.