PolyOne Geon® 1410XX8OFRD Vinyl Compound - Wire & Cable
Subcategory: Polymer; Thermoplastic; Vinyl
Material Notes:
UL 105 C wire & cable insulation compound. THHN,THWN,THW,MTW,UL STYLES 1015,1007 and NMB insulation. PolyOne First Choice Information provided by PolyOne Corporation.
Physical Properties | Original Value | Comments |
|
Specific Gravity | 1.39 g/cc | ASTM D792 |
Mechanical Properties |
|
Hardness, Shore A | 91 | 15 sec; ASTM D2240 |
Tensile Strength, Yield | 3100 psi | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Elongation at Break | 280 % | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Electrical Properties |
|
Volume Resistivity | 1e+015 ohm-cm | ASTM D257 |
Thermal Properties |
|
Brittleness Temperature | -12 °F | ASTM D746 |
Oxygen Index | 31.7 % | 0.075 in; ASTM D2863 |
Processing Properties |
|
Melt Temperature | 350 - 365 °F | Extrusion |
Descriptive Properties | |
Oven Aged - Retention of Elongation (ROE) | 95 % | 277°F (136°C), 168 hrs (7 days), 0.020 in; UL Standard |
Oven Aged - Retention of Tensile Strength (ROT) | 80 % | 277°F (136°C), 168 hrs (7 days), 0.020 in; UL Standard |
|