PolyOne Geon® 1430-xx07FRD Vinyl Compound - Wire & Cable
Subcategory: Polymer; Thermoplastic; Vinyl
Material Notes:
Description/Features: - UL 105°C
- Mil-W-16878
- Meets UL Style 1061 requirements
- CSA-SR
- Flame Retardant
Applications: - Apparatus & Cord Jacket
- Apparatus & Cord Insulation
Market: Processing Method: PolyOne First ChoiceDisclaimer: NOTE: Typical Properties of Molded Slab (0.075"); Not to be Construed as Specifications. Information provided by PolyOne Corporation.
Physical Properties | Original Value | Comments |
|
Specific Gravity | 1.35 g/cc | ASTM D792 |
Mechanical Properties |
|
Hardness, Shore A | 95 | 15 sec; ASTM D2240 |
Hardness, Shore D | 46 | 15 sec; ASTM D2240 |
Tensile Strength, Yield | 3200 psi | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Elongation at Break | 180 % | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Electrical Properties |
|
Volume Resistivity | 1.5e+015 ohm-cm | ASTM D257 |
Thermal Properties |
|
Oxygen Index | 30 % | 0.075 in; ASTM D2863 |
Processing Properties |
|
Melt Temperature | 350 - 370 °F | Extrusion |
Descriptive Properties | |
Oven Aged - Retention of Elongation (ROE) | 90 % | 277°F (136°C), 168 hrs (7 days), 0.075 in; UL Standard |
Oven Aged - Retention of Tensile Strength (ROT) | 95 % | 277°F (136°C), 168 hrs (7 days), 0.075 in; UL Standard |
Product Form | Pellets/Cubes | |
|
Printer friendly version |
|