MatWeb, The Online Materials Database
Aluminum, Al
Subcategory: Aluminum Alloy; Metal; Nonferrous Metal; Pure Element
Close Analogs: Over 1175 Al alloys are listed in MatWeb. Aluminum 1199 is the highest purity (99.99% Al min.) commercially available in structural form.
| Component | Wt. % |  | | | Al | 100 | |
|
Material Notes: This listing is for pure aluminum.
| Physical Properties | Metric | English | Comments |
|
| Density | 2.6989 g/cc | 0.0975 lb/in³ | |
Mechanical Properties |
|
| Hardness, Vickers | 15 | 15 | Annealed |
| Modulus of Elasticity | 68 GPa | 9860 ksi | |
| Shear Modulus | 25 GPa | 3630 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 2.7e-006 ohm-cm | 2.7e-006 ohm-cm | |
| Magnetic Susceptibility | 6e-007 | 6e-007 | cgs/g |
| Critical Magnetic Field Strength, Oersted | 101.9 - 107.9 | 101.9 - 107.9 | |
| Critical Superconducting Temperature | 1.73 - 1.77 K | 1.73 - 1.77 K | |
Thermal Properties |
|
| Heat of Fusion | 386.9 J/g | 166 BTU/lb | |
| CTE, linear 20°C | 24 µm/m-°C | 13.3 µin/in-°F | over the range 20-100ºC |
| CTE, linear 250°C | 25.5 µm/m-°C | 14.2 µin/in-°F | over the range 20-300ºC |
| CTE, linear 500°C | 27.4 µm/m-°C | 15.2 µin/in-°F | over the range 20-500ºC |
| Specific Heat Capacity | 0.9 J/g-°C | 0.215 BTU/lb-°F | |
| Thermal Conductivity | 210 W/m-K | 1460 BTU-in/hr-ft²-°F | |
| Melting Point | 660.37 °C | 1220 °F | |
Optical Properties |
|
| Emissivity (0-1) | 0.2 - 0.3 | 0.2 - 0.3 | strongly oxidized |
| Emissivity (0-1) | 0.05 | 0.05 | polished 50-500ºC |
| Reflection Coefficient, Visible (0-1) | 0.9 | 0.9 | tungsten light |
Descriptive Properties | |
| CAS Number | 7429-90-5 | |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |