Cobalt, Co
Subcategory: Metal; Nonferrous Metal; Pure Element
| Component | Wt. % |  | | | Co | 100 | |
|
| Physical Properties | Original Value | Comments |
|
| Density | 8.8 g/cc | |
Mechanical Properties |
|
| Hardness, Brinell | 125 | |
| Hardness, Vickers | 253 | |
| Tensile Strength, Yield | 225 MPa | |
| Modulus of Elasticity | 211 GPa | |
| Poisson's Ratio | 0.32 | |
| Shear Modulus | 82.6 GPa | |
Electrical Properties |
|
| Electrical Resistivity | 6.24e-006 ohm-cm | |
| Magnetic Permeability | Max 245 | |
| Magnetic Permeability | 68 | Initial |
| Curie Temperature | 1121 °C | |
Thermal Properties |
|
| Heat of Fusion | 259.6 J/g | |
| CTE, linear 20°C | 12.5 µm/m-°C | over the range 20-100ºC |
| CTE, linear 250°C | 14.2 µm/m-°C | at 200°C |
| Specific Heat Capacity | 0.44 J/g-°C | |
| Thermal Conductivity | 69.21 W/m-K | |
| Melting Point | 1493 °C | |
Optical Properties |
|
| Emissivity (0-1) | 0.13 | 500°C unoxidized, total spectrum |
| Reflection Coefficient, Visible (0-1) | 0.37 | 200 nm |
| Reflection Coefficient, Visible (0-1) | 0.675 | 1060 nm |
Descriptive Properties | |
| CAS Number | 7440-48-4 | |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |