Platinum, Pt, CP Grade, Annealed
Subcategory: Metal; Nonferrous Metal; Precious Metal; Pure Element
Component | Wt. % |  | | Pt | 99.95 | |
|
Material Notes: CP Grade (Commercially Pure) is 99.95% pure.
Physical Properties | Metric | English | Comments |
|
Density | 21.45 g/cc | 0.775 lb/in³ | |
Mechanical Properties |
|
Hardness, Vickers | 40 | 40 | |
Tensile Strength, Ultimate | 125 - 165 MPa | 18100 - 23900 psi | |
Elongation at Break | 35 % | 35 % | in 50 mm |
Modulus of Elasticity | 171 GPa | 24800 ksi | static in tension |
Poisson's Ratio | 0.39 | 0.39 | |
Shear Modulus | 62 GPa | 8990 ksi | Calculated value |
Electrical Properties |
|
Electrical Resistivity | 1.06e-005 ohm-cm | 1.06e-005 ohm-cm | Temperature Coefficient of resistivity is 0.0039/K. |
Magnetic Susceptibility | 1.1e-006 | 1.1e-006 | cgs/g |
Thermal Properties |
|
Heat of Fusion | 113 J/g | 48.6 BTU/lb | |
CTE, linear 20°C | 9.1 µm/m-°C | 5.06 µin/in-°F | |
Specific Heat Capacity | 0.134 J/g-°C | 0.032 BTU/lb-°F | |
Thermal Conductivity | 69.1 W/m-K | 480 BTU-in/hr-ft²-°F | |
Melting Point | 1769 °C | 3220 °F | |
Optical Properties |
|
Emissivity (0-1) | 0.152 | 0.152 | at 1000°C for total hemispherical |
Emissivity (0-1) | 0.3 | 0.3 | 650 nm |
Reflection Coefficient, Visible (0-1) | 0.7 | 0.7 | bulk Pt; 589 nm |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |