MatWeb, The Online Materials Database
Platinum, Pt, CP Grade, Annealed
Subcategory: Metal; Nonferrous Metal; Precious Metal; Pure Element
| Component | Wt. % |  | | | Pt | 99.95 | |
|
Material Notes: CP Grade (Commercially Pure) is 99.95% pure.
| Physical Properties | Original Value | Comments |
|
| Density | 21.45 g/cc | |
Mechanical Properties |
|
| Hardness, Vickers | 40 | |
| Tensile Strength, Ultimate | 125 - 165 MPa | |
| Elongation at Break | 35 % | in 50 mm |
| Modulus of Elasticity | 171 GPa | static in tension |
| Poisson's Ratio | 0.39 | |
| Shear Modulus | 62 GPa | Calculated value |
Electrical Properties |
|
| Electrical Resistivity | 1.06e-005 ohm-cm | Temperature Coefficient of resistivity is 0.0039/K. |
| Magnetic Susceptibility | 1.1e-006 | cgs/g |
Thermal Properties |
|
| Heat of Fusion | 113 J/g | |
| CTE, linear 20°C | 9.1 µm/m-°C | |
| Specific Heat Capacity | 0.134 J/g-°C | |
| Thermal Conductivity | 69.1 W/m-K | |
| Melting Point | 1769 °C | |
Optical Properties |
|
| Emissivity (0-1) | 0.152 | at 1000°C for total hemispherical |
| Emissivity (0-1) | 0.3 | 650 nm |
| Reflection Coefficient, Visible (0-1) | 0.7 | bulk Pt; 589 nm |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |