AISI 1018 Steel, cold drawn


Subcategory: AISI 1000 Series Steel; Carbon Steel; Ferrous Metal; Low Carbon Steel; Metal

Key Words: carbon steels, AMS 5069, ASTM A108, UNS G10180, AS 1442 K1018 (Australia), AS 1443 K1018, CSN 12020 (Czech), CSN 12022, AFNOR NF A33-101 AF42C20, DIN 1.0453, DIN C16.8, DGN B-301 1018 (Mexico), COPANT 331 1018 (Pan America), COPANT 333 1018, MST.T (Russia), ST.20A, ST.3, ST.3T, GOST M18S, GOST 23570 18ps, GOST 23570 18sp, GOST 5520 18K, GOST 5521 S, NBN 629 D37-2 (Belgium), NBN 630 E37-1, NBN 630 E37-2, NBN A21-221 C17KD, BDS 9801 S (Bulgaria), GB 715 ML3 (China), TS 302 Fe35.2 (Turkey), TS 346 Fe35, BS 970 080A17, DEF STAN95-1-1 C1018

Component   Wt. %
C0.14 - 0.2 
Fe98.81 - 99.26 
Mn0.6 - 0.9 
PMax 0.04 
SMax 0.05 

Material Notes:
Medium low-carbon steel, has good weldability and slightly better machinability than the lower carbon steels.

Physical PropertiesMetricEnglishComments
Density7.87 g/cc0.284 lb/in³ 

Mechanical Properties
Hardness, Brinell126126 
Hardness, Knoop145145 Converted from Brinell hardness.
Hardness, Rockwell B7171 Converted from Brinell hardness.
Hardness, Vickers131131 Converted from Brinell hardness.
Tensile Strength, Ultimate440 MPa63800 psi 
Tensile Strength, Yield370 MPa53700 psi 
Elongation at Break15 %15 % In 50 mm
Reduction of Area40 %40 % 
Modulus of Elasticity205 GPa29700 ksi Typical for steel
Bulk Modulus140 GPa20300 ksi Typical for steel
Poisson's Ratio0.290.29 Typical For Steel
Machinability70 %70 % Based on AISI 1212 steel. as 100% machinability
Shear Modulus80 GPa11600 ksi Typical for steel

Electrical Properties
Electrical Resistivity1.59e-005 ohm-cm1.59e-005 ohm-cm annealed condition; 0°C (32°F)
Electrical Resistivity at Elevated Temperature2.19e-005 ohm-cm2.19e-005 ohm-cm annealed condition; 100°C (212°F)
Electrical Resistivity at Elevated Temperature2.93e-005 ohm-cm2.93e-005 ohm-cm annealed condition; 200°C (390°F)

Thermal Properties
Specific Heat Capacity0.486 J/g-°C0.116 BTU/lb-°F annealed; 50-100°C (122-212°F)
Thermal Conductivity51.9 W/m-K360 BTU-in/hr-ft²-°F estimated based on similar materials

References are available for this material.

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.