MatWeb, The Online Materials Database
Alclad Aluminum 6061-T6, T651
Subcategory: 6000 Series Aluminum Alloy; Aluminum Alloy; Metal; Nonferrous Metal
Close Analogs: Composition Notes: Composition for AA 6061 (not Alclad 6061 specifically). Aluminum content reported is calculated as remainder. Composition information provided by the Aluminum Association and is not for design.
Key Words: al6061, Alclad 6061-T6, T651; Alclad 6061-T6, T651
| Component | Wt. % |  | | | Al | 95.8 - 98.6 | | | Cr | 0.04 - 0.35 | | | Cu | 0.15 - 0.4 | | | Fe | Max 0.7 | |
| | Component | Wt. % |  | | | Mg | 0.8 - 1.2 | | | Mn | Max 0.15 | | | Other, each | Max 0.05 | | | Other, total | Max 0.15 | |
| | Component | Wt. % |  | | | Si | 0.4 - 0.8 | | | Ti | Max 0.15 | | | Zn | Max 0.25 | |
|
Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.
| Physical Properties | Original Value | Comments |
|
| Density | 2.7 g/cc | For AA6061 (Not Alclad) |
Mechanical Properties |
|
| Ultimate Tensile Strength | 42 ksi | AA; Typical |
| Tensile Yield Strength | 37 ksi | AA; Typical |
| Elongation at Break | 12 % | AA; Typical; 1/16 in. (1.6 mm) Thickness |
| Modulus of Elasticity | 10000 ksi | AA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus. |
| Shear Strength | 27 ksi | AA; Typical |
Processing Properties |
|
| Solution Temperature | 985 °F | |
| Aging Temperature | 320 °F | Rolled or drawn products; hold at temperature for 18 hr |
| Aging Temperature | 350 °F | Extrusions or forgings; hold at temperature for 8 hr |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |