MatWeb, The Online Materials Database
AISI Type 420 Stainless Steel, tested at 205°C (400°F)
Subcategory: Ferrous Metal; Heat Resisting; Metal; Stainless Steel; T 400 Series Stainless Steel
Key Words: UNS S42000, AMS 5506, AMS 5621, ASTM A276, ASTM A314, ASTM A473, ASTM A580, FED QQ-S-763, FED QQ-S-766, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405 (51420), B.S. 420 S 37, B.S. CDS-18 (U.K), martensitic, DIN 1.4021, AFNOR Z 20 C 13 (Fr), UNI X 20 Cr 13, JIS SUS 420 J1, SS14 2303 (Sweden), ISO 683/13 4
| Component | Wt. % |  | | | C | Min 0.15 | | | Cr | 13 | | | Fe | 85 | | | Mn | Max 1 | | | P | Max 0.04 | | | S | Max 0.03 | | | Si | Max 1 | |
|
Material Notes: 16.0 mm diameter bar, austenitized at 980°C for 30 minutes, oil quench, temper for 2 hours at 28°C above test temperature
| Physical Properties | Original Value | Comments |
|
| Density | 7.8 g/cc | |
Mechanical Properties |
|
| Hardness, Brinell | 506 | Converted from Rockwell C Hardness |
| Hardness, Knoop | 562 | Converted from Rockwell C Hardness |
| Hardness, Rockwell C | 51.5 | before testing, 51 after |
| Hardness, Vickers | 541 | Converted from Rockwell C Hardness |
| Tensile Strength, Ultimate | 1820 MPa | |
| Tensile Strength, Yield | 1085 MPa | at 0.2% offset |
| Elongation at Break | 11.5 % | in 50 mm |
| Charpy Impact | 100 J | annealed (tested at room temperature), 14 J quenched and tempered (tested at room temperature) |
| Shear Modulus | 80.7 GPa | |
Electrical Properties |
|
| Electrical Resistivity | 5.5e-005 ohm-cm | at 20°C |
Thermal Properties |
|
| CTE, linear 20°C | 10.3 µm/m-°C | from 0-100°C (32-212°F) |
| CTE, linear 250°C | 10.8 µm/m-°C | at 0-315°C (32-600°F) |
| CTE, linear 500°C | 11.7 µm/m-°C | 0-540°C, 12.2 at 0-650°C |
| Specific Heat Capacity | 0.46 J/g-°C | from 0-100°C (32-212°F) |
| Thermal Conductivity | 24.9 W/m-K | at 100°C |
| Melting Point | 1455 - 1510 °C | |
| Solidus | 1455 °C | |
| Liquidus | 1510 °C | |
| Maximum Service Temperature, Air | 620 °C | Continuous Service |
| Maximum Service Temperature, Air | 735 °C | Intermittent Service |
References are available for this material.
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |