Quadrant EPP Duratron® U1000 PEI, Polyetherimide, unfilled, extruded
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Formerly SABIC Innovative Plastics Ultem® 1000 PEI.
Key Words: Quadrant Engineering Plastics Products; PEI
Material Notes: Duratron® U1000 polyetherimide is an amorphous, high-performance polymer with exceptional flame and heat resistance. It performs continuously to 340°F (171°C), making it ideal for high strength/high heat applications, and those requiring consistent dielectric properties over a wide frequency range. It is hydrolysis resistant, highly resistant to acidic solutions and capable of withstanding multiple autoclaving cycles. Duratron® U1000 is FDA and USP Class VI compliant. FDA compliant colors of Duratron® PEI are also available on a custom basis. Duratron® PEI commonly is machined into parts for reusable medical devices, analytical instrumentation, electrical/electronic insulators and a variety of structural components requiring high strength and rigidity at elevated temperatures. Data provided by Quadrant Engineering Plastic Products from tests on stock shapes and parts produced by Quadrant EPP.
| Physical Properties | Metric | English | Comments |
|
| Specific Gravity | 1.28 g/cc | 0.0462 lb/in³ | ASTM D792 |
| Water Absorption | 0.25 % | 0.25 % | Immersion, 24hr; ASTM D570(2) |
| Water Absorption at Saturation | 1.25 % | 1.25 % | Immersion; ASTM D570(2) |
Mechanical Properties |
|
| Hardness, Rockwell M | 112 | 112 | ASTM D785 |
| Hardness, Rockwell R | 125 | 125 | ASTM D785 |
| Hardness, Shore D | 86 | 86 | ASTM D2240 |
| Tensile Strength, Ultimate | 117 MPa | 17000 psi | ASTM D638 |
| Elongation at Break | 60 % | 60 % | ASTM D638 |
| Tensile Modulus | 3.45 GPa | 500 ksi | ASTM D638 |
| Flexural Modulus | 3.45 GPa | 500 ksi | ASTM D790 |
| Flexural Yield Strength | 138 MPa | 20000 psi | ASTM D790 |
| Compressive Strength | 152 MPa | 22000 psi | 10% Def.; ASTM D695 |
| Compressive Modulus | 3.31 GPa | 480 ksi | ASTM D695 |
| Shear Strength | 103 MPa | 15000 psi | ASTM D732 |
| Coefficient of Friction | 0.42 | 0.42 | Dry vs. Steel; QTM55007 |
| K (wear) Factor | 5840 x 10-8 mm³/N-M | 2900 x 10-10 in³-min/ft-lb-hr | QTM 55010 |
| Limiting Pressure Velocity | 0.0657 MPa-m/sec | 1875 psi-ft/min | 4:1 safety factor; QTM 55007 |
| Izod Impact, Notched | 0.267 J/cm | 0.5 ft-lb/in | ASTM D256 Type A |
Electrical Properties |
|
| Surface Resistivity per Square | Min 1e+013 ohm | Min 1e+013 ohm | EOS/ESD S11.11 |
| Dielectric Constant | 3.15 | 3.15 | 1MHz; ASTM D150 |
| Dielectric Strength | 32.7 kV/mm | 830 V/mil | Short Term; ASTM D149 |
| Dissipation Factor | 0.0013 | 0.0013 | 1MHz; ASTM D150 |
Thermal Properties |
|
| CTE, linear 68°F | 55.8 µm/m-°C | 31 µin/in-°F | (-40°F to 300°F); ASTM E831 |
| Thermal Conductivity | 0.177 W/m-K | 1.23 BTU-in/hr-ft²-°F | ASTM F433 |
| Maximum Service Temperature, Air | 171 °C | 340 °F | Long Term |
| Deflection Temperature at 1.8 MPa (264 psi) | 204 °C | 400 °F | ASTM D648 |
| Glass Temperature | 210 °C | 410 °F | ASTM D3418 |
| Flammability, UL94 | V-0 | V-0 | 1/8 inch |
Descriptive Properties | |
| Compliance - FDA | Compliant | |
| Machinability | 3 | 1-10, 1=Easier to Machine |
| Service in Alcohols | Acceptable | |
| Service in Aliphatic Hydrocarbons | Limited | |
| Service in Aromatic Hydrocarbons | Unacceptable | |
| Service in Chlorinated Solvents | Unacceptable | |
| Service in Ethers | Acceptable | |
| Service in Ketones | Unacceptable | |
| Service in Strong Acids | Unacceptable | |
| Service in Strong Alkalies | Unacceptable | |
| Service in Sunlight | Acceptable | |
| Service in Weak Acids | Acceptable | |
| Service in Weak Alkalies | Acceptable | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |