Advanced Elastomer Systems Santoprene® 121-62 M100 Thermoplastic Rubber


Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A black thermoplastic high-flow elastomer for excellent injection molding performance with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and high quality SEBS compounds. It is polyolefin-based and UV stable.

Key Features: Fast, easy injection molding, especially for complex part geometries; Good sealing performance; Excellent surface aspect; Excellent elastic recovery up to 100°C (212°F); Minimal part warpage; Can be injected at lower molding temperatures or at lower injection pressures

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Physical PropertiesOriginal ValueComments
Density0.91 g/cc TPE-0105 (ASTM D792)

Mechanical Properties
Hardness, Shore A62 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate5 MPa TPE-0153 (ASTM D 412)
Elongation at Break340 % TPE-0153 (ASTM D 412)
100% Modulus0.0021 GPa TPE-0153 (ASTM D 412)
Compression Set28 % 23°C, 168 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature35 % 70°C for 168 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature43 % 100°C, 168 hrs.; TPE-0016 (ASTM D 412)
Tensile Set10 % 23°C, 168 hrs.; TPE-0053 (ASTM D 412)

Thermal Properties
Brittleness TemperatureMax -60 °C TPE-0089 (ASTM D 746)

Processing Properties
Processing Temperature177 - 232 °C 
Drying Temperature82 °C Desiccant drying for 3 hours recommended
Dry Time3 hour 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.