Advanced Elastomer Systems Santoprene® 121-68 W228 Thermoplastic Rubber


Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A black thermoplastic elastomer with good fluid resistance, formulated to replace foamed thermoset elastomers such as EPDM and polychloroprene. It can be processed using extrusion.

Key Features: Continuous temperature rating 1000 hrs. @ 135°C (275°F); Excellent flex fatigue resistance; Excellent ozone resistance; Flexible to -60°C (-76°F). Load Deflection for 150 mm (6") sample is 390 g per ASTM D 1056, 25%, 50 mm/min.

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for extrusion. For mechanical foaming, a 30:1 extruder is recommended. See patent 5,070,111 for more information. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Physical PropertiesMetricEnglishComments
Density0.96 g/cc0.0347 lb/in³ TPE-0105 (ASTM D792)
Apparent Bulk Density0.16 g/cc0.00578 lb/in³ Foamed Density; ASTM D792

Mechanical Properties
Hardness, Shore A6868 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate0.14 MPa20.3 psi Foamed; ASTM D 412
Elongation at Break100 %100 % TPE-0153 (ASTM D 412)
100% Modulus0.00014 GPa0.0203 ksi TPE-0153 (ASTM D 412)
Compression Set9.1 %9.1 % 23°C, 22 hrs. @ 50% deflection; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature46.8 %46.8 % 100°C, 22 hrs. @ 50% deflection; TPE-0016 (ASTM D 412)

Processing Properties
Drying Temperature82 °C180 °F Desiccant drying for 3 hours recommended
Dry Time3 hour3 hour 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.