Advanced Elastomer Systems Santoprene® 201-80 Thermoplastic Rubber


Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A colorable thermoplastic general purpose elastomer with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. It can be processed using injection molding, extrusion, blow molding or other melt processing techniques.

Key Features: Dielectric constant 2.3, dielectric strength at 3.17 mm (125 mil), 19.6 kV/mm (500 v/mil); UL Yellow Card listed, UL 94 HB flame rating; Continuous temperature rating 1000 hrs. @ 135°C (275°F); Excellent flex fatigue resistance; Excellent ozone resistance

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Physical PropertiesMetricEnglishComments
Density0.97 g/cc0.035 lb/in³ TPE-0105 (ASTM D792)

Mechanical Properties
Hardness, Shore A8080 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate11.3 MPa1640 psi TPE-0153 (ASTM D 412)
Elongation at Break520 %520 % TPE-0153 (ASTM D 412)
100% Modulus0.0046 GPa0.667 ksi TPE-0153 (ASTM D 412)
Tear Strength34 kN/m194 pli 34 kN/m at 23°C. Value at 100°C is 13.1 kN/m. TPE-0056 (ASTM D 624)
Compression Set29 %29 % 23°C, 168 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature41 %41 % 100°C, 168 hrs.; TPE-0016 (ASTM D 412)
Tensile Set20 %20 % 23°C, 168 hrs.; TPE-0053 (ASTM D 412)

Electrical Properties
Dielectric Constant2.32.3 Frequency not specified
Dielectric Strength19.6 kV/mm498 kV/in at 3.17 mm (0.125 in)

Thermal Properties
Maximum Service Temperature, Air135 °C275 °F Continuous temperature Rating, 1000 hours
Brittleness TemperatureMax -60 °CMax -76 °F TPE-0089 (ASTM D 746)
Flammability, UL94HBHB 

Processing Properties
Processing Temperature177 - 232 °C351 - 450 °F 
Drying Temperature82 °C180 °F Desiccant drying for 3 hours recommended
Dry Time3 hour3 hour 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.