Advanced Elastomer Systems Santoprene® 211-45 Thermoplastic Rubber


Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A colorable thermoplastic molding grade elastomer with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. A high-flow material designed for use in difficult injection molding applications.

Key Features: Dielectric constant 2.3, dielectric strength at 3.17 mm (125 mil), 19.6 kV/mm (500 v/mil); Excellent flex fatigue resistance; Excellent ozone resistance; Flex modulus at Tangent 5.5 MPa (800 psi); Excellent sealing properties

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Physical PropertiesMetricEnglishComments
Density0.96 g/cc0.0347 lb/in³ TPE-0105 (ASTM D792)

Mechanical Properties
Hardness, Shore A4545 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate3.8 MPa551 psi TPE-0153 (ASTM D 412)
Elongation at Break330 %330 % TPE-0153 (ASTM D 412)
100% Modulus0.0015 GPa0.218 ksi TPE-0153 (ASTM D 412)
Flexural Modulus0.0055 GPa0.798 ksi Tangent
Tear Strength13.7 kN/m78.2 pli at 23°C. Value at 100°C is 4.9 kN/m. TPE-0056 (ASTM D 624)
Compression Set13 %13 % 23°C, 22 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature22 %22 % 100°C, 22 hrs.; TPE-0016 (ASTM D 412)
Tensile Set5 %5 % 23°C, 22 hrs.; per TPE-0053 (ASTM D 412)

Electrical Properties
Dielectric Constant2.32.3 Frequency not specified
Dielectric Strength19.6 kV/mm498 kV/in at 3.17 mm (0.125 in)

Thermal Properties
Brittleness TemperatureMax -60 °CMax -76 °F TPE-0089 (ASTM D 746)

Processing Properties
Processing Temperature177 - 232 °C351 - 450 °F 
Drying Temperature82 °C180 °F Desiccant drying for 3 hours recommended
Dry Time3 hour3 hour 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.