Advanced Elastomer Systems Santoprene® 221-64 W175 Thermoplastic Rubber


Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A colorable thermoplastic UV grade elastomer designed for thin wall extrusion applications with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. It can be processed using extrusion or other melt processing techniques.

Key Features: Dielectric constant 2.3, dielectric strength at 3.17 mm (125 mil), 19.6 kV/mm (500 v/mil); Continuous temperature rating 1000 hrs. @ 135°C (275°F); Excellent flex fatigue resistance; Excellent ozone resistance; Excellent mechanical properties retention after UV exposure; Extrudes thin sections with excellent definition (down to 0.33 mm [1.3"] radius). Long runs with minimal build-up of material on screen packs or narrow die sections.

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Physical PropertiesOriginal ValueComments
Density0.97 g/cc TPE-0105 (ASTM D792)

Mechanical Properties
Hardness, Shore A64 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate6.7 MPa TPE-0153 (ASTM D 412)
Elongation at Break430 % TPE-0153 (ASTM D 412)
100% Modulus0.0024 GPa TPE-0153 (ASTM D 412)
Graves Tear Strength24.5 kN/m TPE-0056 (ASTM D 624)
Compression Set27 % 23°C, 168 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature38 % 100°C, 168 hrs.; TPE-0016 (ASTM D 412)
Tensile Set8.8 % 23°C, 168 hrs.; TPE-0053 (ASTM D 412)

Electrical Properties
Dielectric Constant2.3 Frequency not specified
Dielectric Strength19.6 kV/mm at 3.17 mm (0.125 in)

Thermal Properties
Maximum Service Temperature, Air135 °C Continuous temperature Rating, 1000 hours
Brittleness TemperatureMax -60 °C TPE-0089 (ASTM D 746)

Processing Properties
Processing Temperature177 - 232 °C 
Drying Temperature82 °C Desiccant drying for 3 hours recommended
Dry Time3 hour 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.