BASF Ultraform N 2640 Z4 UNC Q600 Acetal
Subcategory: Acetal; Polymer; Thermoplastic
Material Notes: Information provided by BASF Corporation.
Physical Properties | Metric | English | Comments |
|
Density | 1.35 g/cc | 0.0488 lb/in³ | ISO 1183 |
Water Absorption | 0.8 % | 0.8 % | ISO 62 |
Moisture Absorption at Equilibrium | 0.25 % | 0.25 % | 23°C/50% R.H.; ISO 62 |
Linear Mold Shrinkage | 0.0179 cm/cm | 0.0179 in/in | ISO Data; Parallel to Flow |
Linear Mold Shrinkage | 0.019 cm/cm | 0.019 in/in | MD; ASTM Test |
Linear Mold Shrinkage, Transverse | 0.0182 cm/cm | 0.0182 in/in | ISO Data |
Melt Flow | 5.5 g/10 min | 5.5 g/10 min | 190°C/2.16 kg; ISO 1133 |
Mechanical Properties |
|
Tensile Strength, Yield | 44 MPa | 6380 psi | 2 in/min; ASTM D638 |
Tensile Strength, Yield | 44 MPa | 6380 psi | 50 mm/min; ISO 527 |
Elongation at Break | Min 50 % | Min 50 % | 50 mm/min; Nominal; ISO 527 |
Elongation at Yield | 14 % | 14 % | 50 mm/min; ISO 527 |
Elongation at Yield | 14 % | 14 % | 2 in/min; ASTM D638 |
Tensile Modulus | 1.66 GPa | 241 ksi | ASTM D638 |
Tensile Modulus | 1.7 GPa | 247 ksi | 1 mm/min; ISO 527 |
Flexural Modulus | 1.66 GPa | 241 ksi | ASTM D790 |
Charpy Impact Unnotched | NB | NB | ISO 179 |
Charpy Impact, Notched, Low Temp | 0.8 J/cm² | 3.81 ft-lb/in² | at -30°C; ISO 179 |
Charpy Impact, Unnotched Low Temp | 30 J/cm² | 143 ft-lb/in² | at -30°C; ISO 179 |
Charpy Impact, Notched | 1.3 J/cm² | 6.19 ft-lb/in² | ISO 179 |
Tensile Creep Modulus, 1 hour | 1350 MPa | 196000 psi | ISO 899 |
Tensile Creep Modulus, 1000 hours | 1000 MPa | 145000 psi | ISO 899 |
Izod Impact, Notched @ -40°C | 0.907 J/cm | 1.7 ft-lb/in | ASTM D256 |
Izod Impact, Notched | 0.0149 J/cm | 0.0279 ft-lb/in | ASTM D256 |
Electrical Properties |
|
Volume Resistivity | 1e+011 ohm-cm | 1e+011 ohm-cm | IEC 60093 |
Surface Resistance | 1e+014 ohm | 1e+014 ohm | IEC 60093 |
Dielectric Constant | 4.2 | 4.2 | 100 Hz; IEC 60250 |
Dielectric Constant | 4.2 | 4.2 | 1 MHz; IEC 60250 |
Dielectric Strength | 40 kV/mm | 1020 kV/in | IEC 60243-1 |
Dissipation Factor | 0.011 | 0.011 | 100 Hz; IEC 60250 |
Dissipation Factor | 0.019 | 0.019 | 1 MHz; IEC 60250 |
Comparative Tracking Index | 600 V | 600 V | IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 130 µm/m-°C | 72.2 µin/in-°F | Parallel; ISO 11359 |
CTE, linear 20°C | 70 µm/m-°C | 38.9 µin/in-°F | ASTM E831 |
Melting Point | 167 °C | 333 °F | ASTM D3418 |
Melting Point | 167 °C | 333 °F | 10 K/min |
Deflection Temperature at 0.46 MPa (66 psi) | 140 °C | 284 °F | ASTM D648 |
Deflection Temperature at 0.46 MPa (66 psi) | 140 °C | 284 °F | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 75 °C | 167 °F | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 77 °C | 171 °F | ASTM D648 |
Vicat Softening Point | 130 °C | 266 °F | (50 °C/h / 50N) - B/50; ISO 306 |
Flammability, UL94 | HB | HB | 1.5 mm |
Flammability, UL94 | HB | HB | 3.0 mm |
Descriptive Properties | |
Color | Natural | |
Commercial Status (March 2007) | Active America | |
Impact Modified | Yes | |
Primary Processing Technique | Injection Molding | |
|
|
|
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
|