BASF Ultraform W 2320 003 BK120 Q600 Acetal
Subcategory: Acetal; Polymer; Thermoplastic
Material Notes: Information provided by BASF Corporation.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.4 g/cc | 0.0506 lb/in³ | ISO 1183 |
| Water Absorption | 0.8 % | 0.8 % | ISO 62 |
| Moisture Absorption at Equilibrium | 0.2 % | 0.2 % | 23°C/50% R.H.; ISO 62 |
| Linear Mold Shrinkage | 0.019 cm/cm | 0.019 in/in | MD; ASTM Test |
Mechanical Properties |
|
| Tensile Strength, Yield | 63 MPa | 9140 psi | 50 mm/min; ISO 527 |
| Elongation at Yield | 7.5 % | 7.5 % | 50 mm/min; ISO 527 |
| Tensile Modulus | 2.7 GPa | 392 ksi | 1 mm/min; ISO 527 |
| Flexural Modulus | 2.6 GPa | 377 ksi | ISO 178 |
| Izod Impact, Notched (ISO) | 5.5 kJ/m² | 2.62 ft-lb/in² | ISO 180 |
| Charpy Impact, Notched | 0.55 J/cm² | 2.62 ft-lb/in² | ISO 179 |
Thermal Properties |
|
| Melting Point | 167 °C | 333 °F | ASTM D3418 |
| Melting Point | 167 °C | 333 °F | 10 K/min |
| Deflection Temperature at 1.8 MPa (264 psi) | 90 °C | 194 °F | ISO 75 |
Descriptive Properties | |
| Color | BK120 | |
| Commercial Status (March 2007) | Active America | |
| FDA | 21 CFR 177.2470 | |
| Impact Modified | No | |
| Primary Processing Technique | Injection Molding | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |