MatWeb, The Online Materials Database

Arkema Rilsan® AMN D Nylon 12, Rigid, Injection Grade (Dry)


Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic

Close Analogs:
Arkema, formed in 2004, was formerly Atofina Chemicals and before that Elf Atochem.

Key Words: PA12; Polyamide 12

Material Notes:
Designation ISO 1874-PA12,MR,14-010

Rigid grade for injection molding. Available colors: black, natural, orange, red and white. Possibilities of heat and light stabilizing agents. mold-release agent.

Good mechanical properties. Low friction coefficient. Easy filling of the mold due to its well adapted melt viscosity. Low shrinkage: include 1% on average for the design of the mold. Very good dimensional stability (low moisture absorption). High rate of production.

UL classification: UL94 V2 (3,05mm) RTI(C) 65/65/65

Example applications: Stressed mechanical parts in all industrial field.

ISO data provided by the manufacturer, Arkema.

Physical PropertiesMetricEnglishComments
Density1.01 g/cc0.0365 lb/in³ 
Water Absorption1.6 %1.6 % 
Melt Flow69.4 g/10 min69.4 g/10 min 235°C/2.16 kg load

Mechanical Properties
Tensile Strength, Yield42 MPa6090 psi 50 mm/min
Elongation at BreakMin 50 %Min 50 % Nominal Strain; 50 mm/min
Elongation at Yield8 %8 % 50 mm/min
Tensile Modulus1.45 GPa210 ksi 1 mm/min

Electrical Properties
Dissipation Factor0.0003060.000306 1 MHz
Dissipation Factor, Low Frequency0.0003840.000384 100 Hz

Thermal Properties
Melting Point174 °C345 °F 10°C/min
Flammability, UL94HBHB 1.6 mm
Flammability, UL94V-2V-2 3.2 mm
Oxygen Index21 %21 % 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.