MatWeb, The Online Materials Database

Arkema RilsanŽ ASR 30 Nylon 12, 30% Carbon Fiber Filled (Dry)


Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 12; Polymer; Thermoplastic

Close Analogs:
Arkema, formed in 2004, was formerly Atofina Chemicals and before that Elf Atochem.

Key Words: PA12; Polyamide 12

Material Notes:
Designation ISO 1874-PA12,M,16-120,CF30

Rigid grade with carbon fiber filler (30%) for injection molding. Available color: black.

Very high rigidity. High strength-to-weight ratio. Very low shrinkage: include 0,5% on average for the design of the mold. High dimensional stability (low moisture absorption). Antistatic properties.

Example applications: Parts with high mechanical properties and dimensional precision.

ISO data provided by the manufacturer, Arkema.

Physical PropertiesOriginal ValueComments
Density1.15 g/cc 
Melt Flow3 g/10 min 235°C/2.16 kg load

Mechanical Properties
Tensile Strength, Ultimate161 MPa 5 mm/min
Elongation at Break3 % 5 mm/min
Tensile Modulus15 GPa 1 mm/min
Charpy Impact Unnotched6.12 J/cm˛ 
Charpy Impact, Notched, Low Temp0.94 J/cm˛ at -30°C
Charpy Impact, Unnotched Low Temp5.91 J/cm˛ at -30°C
Charpy Impact, Notched1.45 J/cm˛ 

Thermal Properties
Melting Point174 °C 10°C/min
Flammability, UL94HB 3.1 mm
Flammability, UL94HB 1.6 mm

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.