MatWeb, The Online Materials Database

Bayer MaterialScience Desmopan® 453 Urethane Thermoplastic Elastomer


Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic

Key Words: TPU

Material Notes:
Key Features:

  • Unfilled

Suitable processing methods:

  • Injection molding

Information provided by Bayer Polymers.

Physical PropertiesMetricEnglishComments
Density1.22 g/cc0.0441 lb/in³ 

Mechanical Properties
Tensile Strength, Yield12 MPa1740 psi Stress at 50% Strain
Elongation at BreakMin 50 %Min 50 % 

Electrical Properties
Volume Resistivity2.3e+012 ohm-cm2.3e+012 ohm-cm 
Surface Resistance3e+012 ohm3e+012 ohm 
Dielectric Constant4.54.5 1 MHz
Dielectric Constant5.55.5 100 Hz
Dielectric Strength19.7 kV/mm500 kV/in 
Dissipation Factor0.0270.027 100 Hz
Dissipation Factor0.0690.069 1 MHz
Comparative Tracking Index600 V600 V 

Thermal Properties
CTE, linear 20°C163 µm/m-°C90.6 µin/in-°F Parallel
Vicat Softening Point145 °C293 °F 50°C/h 50N

Processing Properties
Melt Temperature210 °C410 °F Injection Molding
Mold Temperature30 °C86 °F Injection Molding
Injection Pressure50 MPa7250 psi 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.