MatWeb, The Online Materials Database

Bayer MaterialScience Texin® 260 Urethane Thermoplastic Elastomer


Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic

Key Words: TPU

Material Notes:
Key Features:

  • Unfilled

Suitable processing methods:

  • Injection molding

Information provided by Bayer Polymers.

Physical PropertiesMetricEnglishComments
Density1.22 g/cc0.0441 lb/in³ 

Mechanical Properties
Tensile Strength, Yield19 MPa2760 psi Stress at 50% Strain
Elongation at BreakMin 50 %Min 50 % 

Thermal Properties
CTE, linear 20°C181 µm/m-°C101 µin/in-°F Parallel
Deflection Temperature at 0.46 MPa (66 psi)60 °C140 °F 
Vicat Softening Point190 °C374 °F 50°C/h 50N
Glass Temperature-15 °C5 °F 10°C/min
Flammability, UL94HBHB 1.5 mm UL Recognized

Processing Properties
Melt Temperature210 °C410 °F Injection Molding
Mold Temperature30 °C86 °F Injection Molding
Injection Pressure45 MPa6530 psi 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.