Bayer MaterialScience Texin® 270 Urethane Thermoplastic Elastomer


Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic

Key Words: TPU

Material Notes:
Key Features:

  • Unfilled

Suitable processing methods:

  • Injection molding

Information provided by Bayer Polymers.

Physical PropertiesMetricEnglishComments
Density1.24 g/cc0.0448 lb/in³ 

Mechanical Properties
Tensile Strength, Yield28 MPa4060 psi Stress at 50% Strain
Elongation at BreakMin 50 %Min 50 % 

Electrical Properties
Volume Resistivity5e+012 ohm-cm5e+012 ohm-cm 
Surface Resistance9e+014 ohm9e+014 ohm 
Dielectric Constant3.93.9 1 MHz
Dielectric Constant4.64.6 100 Hz
Dielectric Strength23.7 kV/mm602 kV/in 
Dissipation Factor0.0290.029 1 MHz
Dissipation Factor0.0310.031 100 Hz

Thermal Properties
CTE, linear 20°C140 µm/m-°C77.8 µin/in-°F Parallel
Deflection Temperature at 0.46 MPa (66 psi)46 °C115 °F 
Vicat Softening Point158 °C316 °F 50°C/h 50N
Glass Temperature0 °C32 °F 10°C/min

Processing Properties
Melt Temperature230 °C446 °F Injection Molding
Mold Temperature35 °C95 °F Injection Molding
Injection Pressure45 MPa6530 psi 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.