Bayer MaterialScience Texin® 285 Urethane Thermoplastic Elastomer
Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic
Key Words: TPU
Material Notes: Key Features: Suitable processing methods: - Injection molding
- Film extrusion
- Profile extrusion
- Sheet extrusion
- Coating
- Blow molding
Information provided by Bayer Polymers.
Physical Properties | Metric | English | Comments |
|
Density | 1.2 g/cc | 0.0434 lb/in³ | |
Mechanical Properties |
|
Tensile Strength, Yield | 5 MPa | 725 psi | Stress at 50% Strain |
Elongation at Break | Min 50 % | Min 50 % | |
Electrical Properties |
|
Volume Resistivity | 8e+009 ohm-cm | 8e+009 ohm-cm | |
Surface Resistance | 5e+011 ohm | 5e+011 ohm | |
Dielectric Constant | 5.6 | 5.6 | 1 MHz |
Dielectric Constant | 6.5 | 6.5 | 100 Hz |
Dielectric Strength | 17.5 kV/mm | 445 kV/in | |
Dissipation Factor | 0.025 | 0.025 | 100 Hz |
Dissipation Factor | 0.06 | 0.06 | 1 MHz |
Thermal Properties |
|
CTE, linear 20°C | 150 µm/m-°C | 83.3 µin/in-°F | Parallel |
Vicat Softening Point | 91 °C | 196 °F | 50°C/h 50N |
Glass Temperature | -42 °C | -43.6 °F | 10°C/min |
Flammability, UL94 | HB | HB | 1.5 mm UL Recognized |
Flammability, UL94 | V-2 | V-2 | 3 mm UL Recognized |
Processing Properties |
|
Melt Temperature | 200 °C | 392 °F | Injection Molding |
Mold Temperature | 30 °C | 86 °F | Injection Molding |
Injection Pressure | 45 MPa | 6530 psi | |
|
|
![](/images/spacer.gif) |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|