MatWeb, The Online Materials Database

DSM Engineering Plastics Stanyl® 46HF5050 (DAM) Nylon 46 50% Glass Reinforced, Heat Stabilized, Flame Retardant, High Flow (North America)


Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 46; Polymer; Thermoplastic

Key Words: Polyamide 46

Material Notes:
Information provided by DSM Engineering Plastics.

Physical PropertiesOriginal ValueComments
Density1.87 g/cc ISO 1183
Moisture Absorption at Equilibrium1.1 % 50% RH / 23°C; Similar to ISO 62

Mechanical Properties
Tensile Strength at Break200 MPa ISO 527-1/-2
Elongation at Break1.5 % ISO 527-1/-2
Tensile Modulus18 GPa ISO 527-1/-2

Thermal Properties
CTE, linear 20°C20 µm/m-°C parallel to flow; ISO 11359-1/-2
CTE, linear 20°C Transverse to Flow80 µm/m-°C ISO 11359-1/-2
Melting Point295 °C ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi)290 °C ISO 75-1/-2
UL RTI, Electrical140 °C 1.5 mm; UL746B
Flammability, UL94V-0 0.4 mm

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.