MatWeb, The Online Materials Database
DSM Engineering Plastics Stanyl® TW200F6 (DAM) Nylon 46 30% Glass Reinforced, Heat Stabilized (North America)
Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 46; Polymer; Thermoplastic
Key Words: Polyamide 46
Material Notes: Information provided by DSM Engineering Plastics.
Physical Properties | Metric | English | Comments |
|
Density | 1.41 g/cc | 0.0509 lb/in³ | ISO 1183 |
Moisture Absorption at Equilibrium | 2.6 % | 2.6 % | 50% RH / 23°C; Similar to ISO 62 |
Mechanical Properties |
|
Tensile Strength at Break | 210 MPa | 30500 psi | ISO 527-1/-2 |
Elongation at Break | 4 % | 4 % | ISO 527-1/-2 |
Tensile Modulus | 10 GPa | 1450 ksi | ISO 527-1/-2 |
Charpy Impact Unnotched | 8 J/cm² | 38.1 ft-lb/in² | ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 1 J/cm² | 4.76 ft-lb/in² | at -30°C; ISO 179/1eU |
Charpy Impact, Unnotched Low Temp | 7 J/cm² | 33.3 ft-lb/in² | at -30°C; ISO 179/1eU |
Charpy Impact, Notched | 1.2 J/cm² | 5.71 ft-lb/in² | ISO 179/1eU |
Electrical Properties |
|
Volume Resistivity | 1e+012 ohm-cm | 1e+012 ohm-cm | IEC 60093 |
Dielectric Strength | 30 kV/mm | 762 kV/in | IEC 60243-1 |
Comparative Tracking Index | 300 V | 300 V | IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 20 µm/m-°C | 11.1 µin/in-°F | parallel to flow; ISO 11359-1/-2 |
CTE, linear 20°C Transverse to Flow | 80 µm/m-°C | 44.4 µin/in-°F | ISO 11359-1/-2 |
Melting Point | 295 °C | 563 °F | ISO 11357-1/-3 |
Deflection Temperature at 1.8 MPa (264 psi) | 290 °C | 554 °F | ISO 75-1/-2 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |