MatWeb, The Online Materials Database

DuPont Zytel® 153HSL NC010 Nylon 612


Subcategory: Nylon; Nylon 612; Polymer; Thermoplastic

Material Notes:
Zytel® 153HSL NC010 is a heat stabilized, lubricated polyamide 612 resin that is suitable for molding and extrusion.

Physical PropertiesMetricEnglishComments
Density1.06 g/cc0.0383 lb/in³ DAM; ISO 1183
Specific Gravity1.06 g/cc0.0383 lb/in³ DAM; ASTM D 792
Water Absorption0.25 %0.25 % Immersion 24h; 23°C; DAM; ASTM D 570
Moisture Absorption at Equilibrium1.3 %1.3 % 50%RH; 23°C; DAM; ISO 62, Similar to
Water Absorption at Saturation3 %3 % Immersed; 23°C; DAM; ISO 62, Similar to
Water Absorption at Saturation3 %3 % DAM; ASTM D 570
Linear Mold Shrinkage0.011 cm/cm0.011 in/in Flow 3.2mm (0.125in)
Linear Mold Shrinkage0.013 cm/cm0.013 in/in Parallel 2.0mm; ISO 294-4
Linear Mold Shrinkage, Transverse0.014 cm/cm0.014 in/in 2.0mm; ISO 294-4

Mechanical Properties
Hardness, Rockwell R114114 DAM; ASTM D 785
Tensile Strength, Ultimate41 MPa5950 psi 77°C; DAM; ASTM D 638
Tensile Strength, Ultimate61 MPa8850 psi 50%RH; ASTM D 638
Tensile Strength, Ultimate61 MPa8850 psi DAM; ASTM D 638
Tensile Strength, Ultimate94 MPa13600 psi -40°C; 50%RH; ASTM D 638
Tensile Strength, Ultimate94 MPa13600 psi -40°C; DAM; ASTM D 638
Tensile Strength, Yield30 MPa4350 psi 77°C; DAM; ASTM D 638
Tensile Strength, Yield51 MPa7400 psi 50%RH; ASTM D 638
Tensile Strength, Yield53 MPa7690 psi 50%RH; ISO 527
Tensile Strength, Yield61 MPa8850 psi DAM; ASTM D 638
Tensile Strength, Yield62 MPa8990 psi DAM; ISO 527
Tensile Strength, Yield93 MPa13500 psi -40°C; 50%RH; ASTM D 638
Tensile Strength, Yield94 MPa13600 psi -40°C; DAM; ASTM D 638
Elongation at BreakMin 300 %Min 300 % 50%RH; ASTM D 638
Elongation at BreakMin 50 %Min 50 % 50%RH; Nominal; ISO 527
Elongation at Break15 %15 % -40°C; DAM; ASTM D 638
Elongation at Break150 %150 % DAM; ASTM D 638
Elongation at Break30 %30 % -40°C; 50%RH; ASTM D 638
Elongation at Break30 %30 % DAM; Nominal; ISO 527
Elongation at Yield14 %14 % ASTM D 638
Elongation at Yield19 %19 % ISO 527
Elongation at Yield30 %30 % ASTM D 638
Elongation at Yield4.4 %4.4 % ISO 527
Elongation at Yield40 %40 % ASTM D 638
Elongation at Yield7 %7 % ASTM D 638
Elongation at Yield8 %8 % ASTM D 638
Tensile Modulus1.6 GPa232 ksi 50%RH; ISO 527
Tensile Modulus2.4 GPa348 ksi DAM; ISO 527
Flexural Modulus0.41 GPa59.5 ksi 77°C; DAM; ASTM D 790
Flexural Modulus1.24 GPa180 ksi 50%RH; ASTM D 790
Flexural Modulus1.45 GPa210 ksi 50%RH; ISO 178
Flexural Modulus2.03 GPa294 ksi DAM; ASTM D 790
Flexural Modulus2.1 GPa305 ksi DAM; ISO 178
Flexural Modulus2.3 GPa334 ksi -40°C; DAM; ASTM D 790
Flexural Modulus2.8 GPa406 ksi -40°C; 50%RH; ASTM D 790
Shear Strength59 MPa8560 psi DAM; ASTM D 732
Izod Impact, Notched (ISO)4 kJ/m²1.9 ft-lb/in² DAM; ISO 180/1A
Izod Impact, Notched (ISO)6 kJ/m²2.86 ft-lb/in² 50%RH; ISO 180/1A
Izod Impact, Notched, Low Temp (ISO)5 kJ/m²2.38 ft-lb/in² -30°C; DAM; ISO 180/1A
Izod Impact, Notched, Low Temp (ISO)5 kJ/m²2.38 ft-lb/in² -30°C; 50%RH; ISO 180/1A
Charpy Impact UnnotchedNBNB DAM; ISO 179/1eU
Charpy Impact UnnotchedNBNB 50%RH; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.4 J/cm²1.9 ft-lb/in² -30°C; 50%RH; ISO 179/1eA
Charpy Impact, Notched, Low Temp0.5 J/cm²2.38 ft-lb/in² -30°C; DAM; ISO 179/1eA
Charpy Impact, Unnotched Low TempNBNB -30°C; 50%RH; ISO 179/1eU
Charpy Impact, Unnotched Low TempNBNB -30°C; DAM; ISO 179/1eU
Charpy Impact, Notched0.4 J/cm²1.9 ft-lb/in² DAM; ISO 179/1eA
Charpy Impact, Notched0.7 J/cm²3.33 ft-lb/in² 50%RH; ISO 179/1eA
Izod Impact, Notched0.32 J/cm0.599 ft-lb/in -40°C; 50%RH; ASTM D 256
Izod Impact, Notched0.43 J/cm0.806 ft-lb/in -40°C; DAM; ASTM D 256
Izod Impact, Notched0.43 J/cm0.806 ft-lb/in DAM; ASTM D 256
Izod Impact, Notched0.75 J/cm1.41 ft-lb/in 50%RH; ASTM D 256

Electrical Properties
Volume Resistivity1e+011 ohm-cm1e+011 ohm-cm 50%RH; IEC 60093
Volume Resistivity1e+013 ohm-cm1e+013 ohm-cm 50%RH; ASTM D 257
Volume Resistivity1e+013 ohm-cm1e+013 ohm-cm DAM; IEC 60093
Volume Resistivity1e+014 ohm-cm1e+014 ohm-cm DAM; ASTM D 257
Surface Resistance1e+012 ohm1e+012 ohm 50%RH; IEC 60093
Surface Resistance1e+012 ohm1e+012 ohm DAM; IEC 60093
Surface Resistance1e+014 ohm1e+014 ohm 50%RH; ASTM D 257
Surface Resistance1e+015 ohm1e+015 ohm DAM; ASTM D 257
Dielectric Constant3.23.2 1E6 Hz; 23°C; DAM; IEC 60250
Dielectric Constant3.43.4 1E6 Hz; 23°C; 50%RH; IEC 60250
Dielectric Constant3.63.6 1E2 Hz; 23°C; DAM; IEC 60250
Dielectric Constant5.35.3 1E2 Hz; 23°C; 50%RH; IEC 60250
Dielectric Strength21.7 kV/mm551 kV/in 50%RH; 2.0mm; IEC 60243-1
Dielectric Strength22.6 kV/mm574 kV/in DAM; 2.0mm; IEC 60243-1
Dissipation Factor0.0140.014 DAM; 1E2 Hz; IEC 60250
Dissipation Factor0.0160.016 DAM; 1E6 Hz; IEC 60250
Dissipation Factor0.020.02 DAM; 1E6 Hz; ASTM D 150
Dissipation Factor0.020.02 DAM; 1E2 Hz; ASTM D 150
Dissipation Factor0.020.02 DAM; 1E3 Hz; ASTM D 150
Dissipation Factor0.040.04 50%RH; 1E6 Hz; IEC 60250
Dissipation Factor0.10.1 50%RH; 1E2 Hz; IEC 60250
Comparative Tracking IndexMin 600 VMin 600 V DAM; UL 746A
Comparative Tracking Index600 V600 V DAM; IEC 60112

Thermal Properties
CTE, linear 20°C120 µm/m-°C66.7 µin/in-°F DAM; 23 - 55°C (73 - 130°F); Parallel; ISO 11359-1/-2
CTE, linear 20°C90 µm/m-°C50 µin/in-°F DAM; -40 - 23°C (-40 - 73°F); Parallel; ISO 11359-1/-2
CTE, linear 20°C Transverse to Flow120 µm/m-°C66.7 µin/in-°F DAM; 23 - 55°C (73 - 130°F); ISO 11359-1/-2
CTE, linear 20°C Transverse to Flow180 µm/m-°C100 µin/in-°F DAM; 55 - 160°C (130 - 320°F); ISO 11359-1/-2
CTE, linear 20°C Transverse to Flow90 µm/m-°C50 µin/in-°F DAM; -40 - 23°C (-40 - 73°F); ISO 11359-1/-2
CTE, linear 100°C170 µm/m-°C94.4 µin/in-°F DAM; 55 - 160°C (130 - 320°F); Parallel; ISO 11359-1/-2
Melting Point218 °C424 °F DAM; ASTM D 3418
Melting Point218 °C424 °F 10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi)135 °C275 °F DAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi)55 °C131 °F DAM; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)62 °C144 °F DAM; ISO 75-1/-2
Brittleness Temperature-109 °C-164 °F 50%RH; ASTM D 746
Brittleness Temperature-126 °C-195 °F DAM; ASTM D 746
UL RTI, Electrical105 °C221 °F 3.0mm; DAM; UL 746B
UL RTI, Electrical105 °C221 °F 1.5mm; DAM; UL 746B
UL RTI, Electrical65 °C149 °F 0.86mm; DAM; UL 746B
UL RTI, Mechanical with Impact65 °C149 °F 1.5mm; DAM; UL 746B
UL RTI, Mechanical with Impact65 °C149 °F 0.86mm; DAM; UL 746B
UL RTI, Mechanical with Impact65 °C149 °F 3.0mm; DAM; UL 746B
UL RTI, Mechanical without Impact65 °C149 °F 3.0mm; DAM; UL 746B
UL RTI, Mechanical without Impact65 °C149 °F 0.86mm; DAM; UL 746B
UL RTI, Mechanical without Impact65 °C149 °F 1.5mm; DAM; UL 746B
Flammability, UL94HBHB 3.0mm; DAM; IEC 60695-11-10
Flammability, UL94HBHB 3.0mm; DAM; UL94
Flammability, UL94HBHB 1.5mm; DAM; IEC 60695-11-10
Flammability, UL94HBHB 1.5mm; DAM; UL94
Flammability, UL94HBHB 0.86mm; DAM; IEC 60695-11-10
Flammability, UL94HBHB 0.86mm; DAM; UL94
Oxygen Index27 %27 % DAM; ISO 4589-1/-2
Glow Wire Test675 °C1250 °F 1.5mm; DAM; Ignition Temperature; IEC 60695-2-13
Glow Wire Test675 °C1250 °F 0.86mm; DAM; Ignition Temperature; IEC 60695-2-13
Glow Wire Test675 °C1250 °F 1.5mm; DAM; Flammability Index; IEC 60695-2-12
Glow Wire Test700 °C1290 °F 3.0mm; DAM; Ignition Temperature; IEC 60695-2-13
Glow Wire Test825 °C1520 °F 0.86mm; DAM; Flammability Index; IEC 60695-2-12
Glow Wire Test925 °C1700 °F 3.0mm; DAM; Flammability Index; IEC 60695-2-12

Processing Properties
Melt Temperature230 - 290 °C446 - 554 °F 
Melt Temperature250 °C482 °F Optimum
Mold Temperature50 - 90 °C122 - 194 °F 
Mold Temperature70 °C158 °F Optimum
Drying Temperature80 °C176 °F 
Dry Time2 - 4 hour2 - 4 hour Dehumidified Dryer
Moisture ContentMax 0.15 %Max 0.15 % 

Descriptive Properties
AdditiveHeat Stabilizer 
AdditiveLubricant 
AppearanceNatural Color 
DryingRecommended If moisture content of resin exceeds recommended level
DuPont Product CategoryExtrusion Resins 
DuPont Product CategoryUnreinforced Resins 
ExtrudableBlown Film 
ExtrudableCoating 
ExtrudableFilament 
ExtrudableHose 
ExtrudableSheet 
ExtrudableTubing 
ExtrudableWire and Cable 
Extrusion Blow MoldableYes 
FeaturesChemical Resistance, Good 
FeaturesElectrical Properties, Good 
FeaturesHeat Aging Resistance, Good 
FormPellets 
Heat StabilizedYes 
Injection Blow MoldableYes 
Injection MoldableYes 
Part Marking Code>PA612< ISO 11469
Processing MethodExtrusion 
Processing MethodInjection Molding 
RegionAmericas 
RegionAsia/Pacific 
RegionEurope 
Resin IdentificationPA612 ISO 1043
Ultrasonic WeldableYes 
UsesAutomotive Applications 
UsesCable Jacketing 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.