MatWeb, The Online Materials Database
DuPont Zytel® 159 NC010 Nylon 612
Subcategory: Nylon; Nylon 612; Polymer; Thermoplastic
Material Notes: Zytel® 159 NC010 is a high viscosity polyamide 612 resin that is suitable for extrusion applications, such as monofilaments and tubing.
| Physical Properties | Original Value | Comments |
|
| Density | 1.06 g/cc | DAM; ISO 1183 |
| Water Absorption | 0.45 % | Immersion 24h; 23°C; DAM; ISO 62, Similar to |
Mechanical Properties |
|
| Tensile Strength, Yield | 62 MPa | DAM; ISO 527 |
| Elongation at Break | 35 % | DAM; Nominal; ISO 527 |
| Elongation at Yield | 4.5 % | ISO 527 |
| Tensile Modulus | 2.4 GPa | DAM; ISO 527 |
| Flexural Modulus | 2.15 GPa | DAM; ISO 178 |
| Charpy Impact, Notched | 0.5 J/cm² | DAM; ISO 179/1eA |
Thermal Properties |
|
| Melting Point | 216 °C | 10°C/min; DAM; ISO 11357-1/-3 |
| Deflection Temperature at 1.8 MPa (264 psi) | 62 °C | DAM; ISO 75-1/-2 |
Processing Properties |
|
| Melt Temperature | 230 - 290 °C | |
| Melt Temperature | 250 °C | Optimum |
| Mold Temperature | 50 - 90 °C | |
| Mold Temperature | 70 °C | Optimum |
| Drying Temperature | 80 °C | |
| Dry Time | 2 - 4 hour | Dehumidified Dryer |
| Moisture Content | Max 0.05 % | |
Descriptive Properties | |
| Drying | Recommended | If moisture content of resin exceeds recommended level |
| DuPont Product Category | Extrusion Resins | |
| DuPont Product Category | Unreinforced Resins | |
| Form | Pellets | |
| Region | Americas | |
| Region | Asia/Pacific | |
| Region | Europe | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |