SABIC Innovative Plastics CYCOLOY C6600 ABS + Polycarbonate (North America)
Subcategory: ABS Polymer; Polycarbonate; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Original Value | Comments |
|
| Density | 1.19 g/cc | ASTM D 792 |
| Water Absorption | 0.11 % | 24 hours @ 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.004 - 0.006 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 21.5 g/10 min | 260C/2.16 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 7100 psi | Type I, 2.0 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 9200 psi | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Break | 80 % | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Yield | 4 % | Type I, 2.0 in/min; ASTM D 638 |
| Tensile Modulus | 435000 psi | 2.0 in/min; ASTM D 638 |
| Flexural Modulus | 380000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Yield Strength | 13700 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Gardner Impact @ 23°C | 450 in-lb | Instrumented Impact Total Energy, 73°F; ASTM D 3763 |
| Gardner Impact @ 23°C | 450 in-lb | Instrumented Impact Total Energy, -22F; ASTM D 3763 |
| Izod Impact, Notched | 11 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | Min 1e+015 ohm-cm | IEC 60093 |
| Surface Resistivity per Square | Min 1e+015 ohm | IEC 60093 |
| Dielectric Constant | 2.7 | 50 Hz; IEC 60250 |
| Dielectric Constant | 2.7 | 1 MHz; IEC 60250 |
| Dielectric Strength | 17 kV/mm | in oil, 3.2 mm; IEC 60243-1 |
| Dissipation Factor | 0.004 | 50 Hz; IEC 60250 |
| Dissipation Factor | 0.006 | 1 MHz; IEC 60250 |
| Comparative Tracking Index | 600 V | IEC 112/3rd |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 208 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 194 °F | 0.125 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 211 °F | Rate B; ASTM D 1525 |
| UL RTI, Electrical | 80 °C | UL 746B |
| UL RTI, Mechanical with Impact | 70 °C | UL 746B |
| UL RTI, Mechanical without Impact | 80 °C | UL 746B |
| Flammability, UL94 | V-2 | 0.03 in. |
| Flammability, UL94 | V-0 | 0.059 in. |
| Flammability, UL94 | 6 | 0.079 in. |
Descriptive Properties | |
| UL File Number, GLOBAL | E161759 | |
| UL File Number, USA | E121562 | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from