| Physical Properties | Metric | English | Comments |
|
| Density | 1.26 g/cc | 0.0455 lb/in³ | ASTM D 792 |
| Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | 0.005 - 0.007 in/in | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 24 g/10 min | 24 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 96.5 MPa | 14000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 70 % | 70 % | Type I, 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 3.17 GPa | 460 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 145 MPa | 21000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Unnotched | 20.8 J/cm | 39 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 0.534 J/cm | 1 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 21.4 J/cm | 40 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Comparative Tracking Index | 100 - 175 V | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | Min 120 sec | Min 120 sec | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Amp Arc Ignition, HAI | Max 15 arcs | Max 15 arcs | Surface (+/- 0.125 inch); PLC Code 4; UL 746A |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 191 °C | 375 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 115 °C | 239 °F | UL 746B |
| UL RTI, Mechanical with Impact | 115 °C | 239 °F | UL 746B |
| UL RTI, Mechanical without Impact | 115 °C | 239 °F | UL 746B |
| Flammability, UL94 | V-2 | V-2 | 0.03 in. |
| Flammability, UL94 | V-0 | V-0 | 0.059 in. |
Descriptive Properties | |
| UL File Number, USA | E121562 | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |