MatWeb, The Online Materials Database
SABIC Innovative Plastics ULTEM HTX1010F Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.26 g/cc | ASTM D 792 |
| Melt Flow | 15.5 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 12000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 13500 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 40 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 450000 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 440000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 20000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Unnotched | 39 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 3 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 33 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 385 °F | 0.250 inch, unannealed; ASTM D 648 |
| Oxygen Index | 39.7 % | ASTM D 2863 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |