MatWeb, The Online Materials Database
SABIC Innovative Plastics ULTEM 1000M Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.27 g/cc | ASTM D 792 |
| Water Absorption | 0.25 % | 24 hours @ 73F; ASTM D 570 |
| Water Absorption at Saturation | 1.25 % | Equilibrium, 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 9.7 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Hardness, Rockwell M | 109 | ASTM D 785 |
| Tensile Strength @ Yield | 16000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 60 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 7 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 520000 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 510000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 24000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Poisson's Ratio | 0.36 | ASTM D 638 |
| Izod Impact, Unnotched | 25 ft-lb/in | 73F; ASTM D 4812 |
| Gardner Impact | 27 ft-lb | 73F; ASTM D 3029 |
| Taber Abrasion, mg/1000 Cycles | 10 | CS-17, 1 kg; ASTM D 1044 |
| Izod Impact, Notched | 1 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 30 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | 1e+017 ohm-cm | ASTM D 257 |
| Dielectric Constant | 3.15 | 1 kHz; ASTM D 150 |
| Dielectric Strength | 710 V/mil | in oil, 62 mils; ASTM D 149 |
| Dielectric Strength | 831 V/mil | in air, 62 mils; ASTM D 149 |
| Dissipation Factor | 0.0013 | 1 kHz; ASTM D 150 |
| Dissipation Factor | 0.0025 | 2450 MHz; ASTM D 150 |
Thermal Properties |
|
| CTE, linear, 212°F (100°C) | 30 µin/in-°F | Cross Flow; 0F to 300F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 31 µin/in-°F | Flow, 0F to 300F; ASTM E 831 |
| Thermal Conductivity | 0.22 W/m-K | ASTM C 177 |
| Deflection Temperature at 0.46 MPa (66 psi) | 410 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 394 °F | 0.250 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 426 °F | Rate B; ASTM D 1525 |
| Flammability, UL94 | V-0 | 0.016 in. |
| NBS Smoke Density | 0.7 | Flaming, Ds 4 min; ASTM E 662 |
| NBS Smoke Density | 30 | Flaming, Dmax 20 min; ASTM E 662 |
| Oxygen Index | 47 % | ASTM D 2863 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |