SABIC Innovative Plastics ULTEM 1010 Polyetherimide (North America)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.

Physical PropertiesOriginal ValueComments
Density1.27 g/cc ASTM D 792
Water Absorption0.25 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation1.25 % Equilibrium, 73F; ASTM D 570
Linear Mold Shrinkage0.005 - 0.007 cm/cm Flow, 0.125 inch; ASTM D 955
Melt Flow17.8 g/10 min 337C/6.6 kgf; ASTM D 1238

Mechanical Properties
Hardness, Rockwell M109 ASTM D 785
Tensile Strength @ Yield16000 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break60 % Type I, 0.2 in/min; ASTM D 638
Elongation at Yield7 % Type I, 0.2 in/min; ASTM D 638
Tensile Modulus520000 psi 0.2 in/min; ASTM D 638
Flexural Modulus510000 psi 0.10 in/min, 4" span; ASTM D 790
Flexural Yield Strength24000 psi 0.10 in/min, 4" span; ASTM D 790
Izod Impact, Unnotched25 ft-lb/in 73F; ASTM D 4812
Gardner Impact25 ft-lb 73F; ASTM D 3029
Taber Abrasion, mg/1000 Cycles10 CS-17, 1 kg; ASTM D 1044
Izod Impact, Notched0.6 ft-lb/in 73F; ASTM D 256
Izod Impact, Notched22 ft-lb/in Reverse Notched, 73F; ASTM D 256

Electrical Properties
Volume Resistivity1e+017 ohm-cm ASTM D 257
Dielectric Constant3.15 1 kHz; ASTM D 150
Dielectric Strength710 V/mil in oil, 62 mils; ASTM D 149
Dielectric Strength830 V/mil in air, 62 mils; ASTM D 149
Dissipation Factor0.0013 1 kHz; ASTM D 150
Dissipation Factor0.0025 2450 MHz; ASTM D 150
Arc Resistance120 - 180 sec Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495
Comparative Tracking Index100 - 175 V (+/- 0.125 inch); PLC Code 4; UL 746A
Hot Wire Ignition, HWI60 - 120 sec (+/- 0.125 inch); PLC Code 1; UL 746A
High Amp Arc Ignition, HAI15 - 30 arcs Surface (+/- 0.125 inch); PLC Code 3; UL 746A
High Voltage Arc-Tracking Rate, HVTR25.4 - 80 mm/min (+/- 0.125 inch); PLC Code 2; UL 746A

Thermal Properties
CTE, linear, 212°F (100°C)31 µin/in-°F Flow, 0F to 300F; ASTM E 831
Thermal Conductivity0.22 W/m-K ASTM C 177
Deflection Temperature at 0.46 MPa (66 psi)405 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)390 °F 0.250 inch, unannealed; ASTM D 648
Vicat Softening Point426 °F Rate B; ASTM D 1525
UL RTI, Electrical170 °C UL 746B
UL RTI, Mechanical with Impact170 °C UL 746B
UL RTI, Mechanical without Impact170 °C UL 746B
Flammability, UL94V-2 0.028 in.
Flammability, UL94V-0 0.028 in.
Flammability, UL947 0.118 in.
NBS Smoke Density2 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density39 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index44 % ASTM D 2863

Descriptive Properties
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.