| Physical Properties | Metric | English | Comments |
|
| Density | 1.34 g/cc | 0.0484 lb/in³ | ASTM D 792 |
| Water Absorption | 0.21 % | 0.21 % | 24 hours @ 73F; ASTM D 570 |
| Water Absorption at Saturation | 1.2 % | 1.2 % | Equilibrium, 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.005 - 0.006 cm/cm | 0.005 - 0.006 in/in | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 7 g/10 min | 7 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Hardness, Rockwell M | 114 | 114 | ASTM D 785 |
| Tensile Strength @ Break | 116 MPa | 16800 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 114 MPa | 16600 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 6 % | 6 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 4.69 GPa | 680 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 5.17 GPa | 750 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Strength | 200 MPa | 29000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Unnotched | 4.81 J/cm | 9 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 0.534 J/cm | 1 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 4.59 J/cm | 8.6 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | 1e+017 ohm-cm | 1e+017 ohm-cm | ASTM D 257 |
| Dielectric Constant | 3.5 | 3.5 | 1 kHz; ASTM D 150 |
| Dielectric Strength | 27.6 kV/mm | 700 V/mil | in oil, 62 mils; ASTM D 149 |
| Dissipation Factor | 0.0014 | 0.0014 | 1 kHz; ASTM D 150 |
| Dissipation Factor | 0.0046 | 0.0046 | 2450 MHz; ASTM D 150 |
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
| Comparative Tracking Index | 100 - 175 V | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
| High Amp Arc Ignition, HAI | Max 15 arcs | Max 15 arcs | Surface (+/- 0.125 inch); PLC Code 4; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80 mm/min | 1 - 3.15 in/min | (+/- 0.125 inch); PLC Code 2; UL 746A |
Thermal Properties |
|
| CTE, linear, 212°F (100°C) | 32.4 µm/m-°C | 18 µin/in-°F | Flow, 0F to 300F; ASTM E 831 |
| Deflection Temperature at 0.46 MPa (66 psi) | 210 °C | 410 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 209 °C | 408 °F | 0.250 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 223 °C | 434 °F | Rate B; ASTM D 1525 |
| UL RTI, Electrical | 170 °C | 338 °F | UL 746B |
| UL RTI, Mechanical with Impact | 170 °C | 338 °F | UL 746B |
| UL RTI, Mechanical without Impact | 170 °C | 338 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.016 in. |
| Flammability, UL94 | 7 | 7 | 0.075 in. |
| NBS Smoke Density | 1.8 | 1.8 | Flaming, Ds 4 min; ASTM E 662 |
| NBS Smoke Density | 27 | 27 | Smolder, Dmax 20 min; ASTM E 662 |
| Oxygen Index | 47 % | 47 % | ASTM D 2863 |
Descriptive Properties |
|
| CSA File No. | LS88480 | |
| UL File Number, USA | E121562 | |