MatWeb, The Online Materials Database

SABIC Innovative Plastics ULTEM 2313 Polyetherimide (North America)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.52 g/cc0.0549 lb/in³ ASTM D 792
Water Absorption0.18 %0.18 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation0.98 %0.98 % Equilibrium, 73F; ASTM D 570
Linear Mold Shrinkage0.003 - 0.004 cm/cm0.003 - 0.004 in/in Flow, 0.125 inch; ASTM D 955
Linear Mold Shrinkage, Transverse0.0045 - 0.0055 cm/cm0.0045 - 0.0055 in/in 0.125 inch; ASTM D 955
Melt Flow9.3 g/10 min9.3 g/10 min 337C/6.6 kgf; ASTM D 1238

Mechanical Properties
Tensile Strength @ Break86.2 MPa12500 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break3 %3 % Type I, 0.2 in/min; ASTM D 638
Flexural Modulus6.96 GPa1010 ksi 0.10 in/min, 4" span; ASTM D 790
Flexural Strength172 MPa25000 psi 0.10 in/min, 4" span; ASTM D 790
Izod Impact, Notched0.32 J/cm0.6 ft-lb/in 73F; ASTM D 256
Izod Impact, Notched2.67 J/cm5 ft-lb/in Reverse Notched, 73F; ASTM D 256

Electrical Properties
Dielectric Constant3.73.7 1 kHz; ASTM D 150
Arc Resistance60 - 120 sec60 - 120 sec Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495
Comparative Tracking Index100 - 175 V100 - 175 V (+/- 0.125 inch); PLC Code 4; UL 746A
Hot Wire Ignition, HWI60 - 120 sec60 - 120 sec (+/- 0.125 inch); PLC Code 1; UL 746A
High Amp Arc Ignition, HAIMax 15 arcsMax 15 arcs Surface (+/- 0.125 inch); PLC Code 4; UL 746A
High Voltage Arc-Tracking Rate, HVTR25.4 - 80 mm/min1 - 3.15 in/min (+/- 0.125 inch); PLC Code 2; UL 746A

Thermal Properties
Deflection Temperature at 1.8 MPa (264 psi)208 °C406 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical105 °C221 °F UL 746B
UL RTI, Mechanical with Impact105 °C221 °F UL 746B
UL RTI, Mechanical without Impact105 °C221 °F UL 746B
Flammability, UL94V-0V-0 0.014 in.

Descriptive Properties
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.