MatWeb, The Online Materials Database

SABIC Innovative Plastics ULTEM 7801 Polyetherimide (North America)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.

Physical PropertiesOriginal ValueComments
Density1.37 g/cc ASTM D 792
Linear Mold Shrinkage0.0015 - 0.003 cm/cm Flow, 0.125 inch; ASTM D 955
Melt Flow2.4 g/10 min 337C/6.6 kgf; ASTM D 1238

Mechanical Properties
Tensile Strength @ Break30000 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break2 % Type I, 0.2 in/min; ASTM D 638
Flexural Modulus2.1e+006 psi 0.10 in/min, 4" span; ASTM D 790
Flexural Yield Strength38000 psi 0.10 in/min, 4" span; ASTM D 790
Izod Impact, Notched1.4 ft-lb/in 73F; ASTM D 256
Izod Impact, Notched7.2 ft-lb/in Reverse Notched, 73F; ASTM D 256

Electrical Properties
Volume Resistivity100000 ohm-cm ASTM D 257
Surface Resistivity per Square10000 ohm ASTM D 257

Thermal Properties
CTE, linear, 212°F (100°C)22 µin/in-°F Cross Flow; 0F to 300F; ASTM E 831
CTE, linear, 212°F (100°C)4 µin/in-°F Flow, 0F to 300F; ASTM E 831
Deflection Temperature at 1.8 MPa (264 psi)417 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical105 °C UL 746B
UL RTI, Mechanical with Impact105 °C UL 746B
UL RTI, Mechanical without Impact105 °C UL 746B
Flammability, UL94V-0 0.058 in.

Descriptive Properties
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.