MatWeb, The Online Materials Database
SABIC Innovative Plastics ULTEM 9075 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Original Value | Comments |
|
| Density | 1.3 g/cc | ASTM D 792 |
| Halogen Content | 0 % | GE Test |
| Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.005 - 0.007 cm/cm | 0.125 inch; ASTM D 955 |
| Melt Flow | 2.4 g/10 min | 295C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 14000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 85 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 480000 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 470000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Strength | 20500 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 21000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Gardner Impact | 26 ft-lb | 73F; ASTM D 3029 |
| Izod Impact, Notched | 1.3 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 39 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 372 °F | 0.250 inch, unannealed; ASTM D 648 |
| Flammability Test | 0 | Vertical Burn, drip time; seconds; FAR 25.853 |
| Flammability Test | 1 | Vertical Burn, extinguish time; seconds; FAR 25.853 |
| Flammability Test | 10 | OSU 2 minute heat, release rate; KW-Min/m2; FAR 25.853 |
| Flammability Test | 5 | Vertical Burn, length; inches; FAR 25.853 |
| NBS Smoke Density | 5 | Flaming, Dmax; FAR 25.853 |
Descriptive Properties | |
| FAR 25.853 | SECT A-1 | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |