MatWeb, The Online Materials Database

SABIC Innovative Plastics VALOX DR51U PBT (North America)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.41 g/cc0.0509 lb/in³ ASTM D 792
Water Absorption0.07 %0.07 % 24 hours @ 73F; ASTM D 570
Linear Mold Shrinkage0.004 - 0.006 cm/cm0.004 - 0.006 in/in Flow, 60-125 mil; ASTM D 955
Linear Mold Shrinkage0.006 - 0.009 cm/cm0.006 - 0.009 in/in Flow, 125-180 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.005 - 0.008 cm/cm0.005 - 0.008 in/in 60-125 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.008 - 0.011 cm/cm0.008 - 0.011 in/in 125-180 mil; ASTM D 955

Mechanical Properties
Hardness, Rockwell R118118 ASTM D 785
Tensile Strength @ Break93.1 MPa13500 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break5 %5 % Type I, 0.2 in/min; ASTM D 638
Flexural Modulus4.83 GPa700 ksi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength145 MPa21000 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched5.34 J/cm10 ft-lb/in 73F; ASTM D 4812
Izod Impact, Notched0.534 J/cm1 ft-lb/in 73F; ASTM D 256

Electrical Properties
Volume Resistivity3.3e+016 ohm-cm3.3e+016 ohm-cm ASTM D 257
Dielectric Constant3.43.4 1 MHz; ASTM D 150
Dielectric Constant3.63.6 100 Hz; ASTM D 150
Dielectric Strength19.7 kV/mm500 V/mil in air, 125 mils; ASTM D 149
Dielectric Strength23.2 kV/mm590 V/mil in oil, 62 mils; ASTM D 149
Dissipation Factor0.0020.002 100 Hz; ASTM D 150
Dissipation Factor0.020.02 1 MHz; ASTM D 150
Arc Resistance120 - 180 sec120 - 180 sec Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495
Comparative Tracking Index250 - 400 V250 - 400 V (+/- 0.125 inch); PLC Code 2; UL 746A
High Voltage Arc-Tracking Rate, HVTR10 - 25.4 mm/min0.394 - 1 in/min (+/- 0.125 inch); PLC Code 1; UL 746A

Thermal Properties
CTE, linear 68°F21.6 µm/m-°C12 µin/in-°F Flow, -40F to 200F; ASTM E 831
CTE, linear, 212°F (100°C)21.6 µm/m-°C12 µin/in-°F Flow, 140F to 280F; ASTM E 831
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)191 °C375 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical130 °C266 °F UL 746B
UL RTI, Mechanical with Impact130 °C266 °F UL 746B
UL RTI, Mechanical without Impact140 °C284 °F UL 746B
Flammability, UL94HBHB 0.028 in.

Descriptive Properties
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.