MatWeb, The Online Materials Database

SABIC Innovative Plastics VALOX FV649 PBT (North America)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.13 g/cc0.0408 lb/in³ Molded Foam; ASTM D 792
Density1.26 g/cc0.0455 lb/in³ ASTM D 792
Water Absorption0.15 %0.15 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation0.33 %0.33 % Equilibrium, 73F; ASTM D 570
Linear Mold Shrinkage0.0035 - 0.0055 cm/cm0.0035 - 0.0055 in/in Flow, 0.250 inch; ASTM D 955

Mechanical Properties
Tensile Strength @ Yield46.9 MPa6800 psi 0.250"; ASTM D 638
Elongation at Break5.4 %5.4 % 0.250"; ASTM D 638
Tensile Modulus3 GPa435 ksi 0.250"; ASTM D 638
Flexural Modulus3.21 GPa465 ksi 0.250"; ASTM D 790
Flexural Yield Strength80.7 MPa11700 psi 0.250"; ASTM D 790
Izod Impact, Unnotched10.7 J/cm20 ft-lb/in 73F; ASTM D 4812
Falling Dart Impact108 J80 ft-lb 73F; GE Test

Electrical Properties
Volume Resistivity1.4e+016 ohm-cm1.4e+016 ohm-cm ASTM D 257
Surface Resistivity per SquareMin 1.1e+017 ohmMin 1.1e+017 ohm ASTM D 257
Dielectric Constant2.712.71 100 Hz; ASTM D 150
Dielectric Constant2.82.8 1 MHz; ASTM D 150
Dielectric Strength12.8 kV/mm326 V/mil in air, 250 mils; ASTM D 149
Dissipation Factor0.00280.0028 100 Hz; ASTM D 150
Dissipation Factor0.03470.0347 1 MHz; ASTM D 150
Arc Resistance60 - 120 sec60 - 120 sec Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495
Comparative Tracking Index100 - 175 V100 - 175 V (+/- 0.125 inch); PLC Code 4; UL 746A
High Voltage Arc-Tracking Rate, HVTR80 - 150 mm/min3.15 - 5.91 in/min (+/- 0.125 inch); PLC Code 3; UL 746A

Thermal Properties
CTE, linear 68°F32.4 µm/m-°C18 µin/in-°F Flow, -40F to 200F; ASTM E 831
Specific Heat Capacity1.34 J/g-°C0.32 BTU/lb-°F ASTM C 351
Deflection Temperature at 0.46 MPa (66 psi)116 °C240 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)108 °C226 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical75 °C167 °F UL 746B
UL RTI, Mechanical with Impact75 °C167 °F UL 746B
UL RTI, Mechanical without Impact75 °C167 °F UL 746B
Flammability, UL94HBHB 0.157 in.
Flammability Test11 FOAM - Flame Class Minimum Density; g/cm3

Descriptive Properties
Foam Weight Reduction10% Mechanical Properties Reported Herein (0.250")
Foam Weight Reduction10% Impact Properties Reported Herein (0.250")
Foam Weight Reduction10% Thermal Properties Reported Herein (0.250")
Foam Weight Reduction10% Physical Properties Reported Herein (0.250")
Foam Weight Reduction20% Electrical Properties Reported Herein (0.250")
UL File Number, USAE121562 
UV-light, water exposure/immersionF2 UL746C

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.