MatWeb, The Online Materials Database
SABIC Innovative Plastics VALOX HF4030 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.51 g/cc | 0.0546 lb/in³ | ASTM D 792 |
| Water Absorption | 0.037 % | 0.037 % | 24 hours @ 73F; ASTM D 570 |
| Viscosity | 470000 cP | 470000 cP | Melt Viscosity; GE Test |
| Linear Mold Shrinkage | 0.005 cm/cm | 0.005 in/in | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.009 cm/cm | 0.009 in/in | 0.125 inch; ASTM D 955 |
Mechanical Properties |
|
| Tensile Strength @ Break | 105 MPa | 15200 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 2 % | 2 % | Type I, 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 7.24 GPa | 1050 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 190 MPa | 27500 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 7.21 J/cm | 13.5 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 0.801 J/cm | 1.5 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | Min 1e+016 ohm-cm | Min 1e+016 ohm-cm | ASTM D 257 |
| Dielectric Constant | 3.1 | 3.1 | 1 MHz; ASTM D 150 |
| Dielectric Strength | 18.5 kV/mm | 471 V/mil | in oil, 125 mils; ASTM D 149 |
| Dissipation Factor | 0.01 | 0.01 | 1 MHz; ASTM D 150 |
| Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | 400 - 600 V | 400 - 600 V | (+/- 0.125 inch); PLC Code 1; UL 746A |
| Hot Wire Ignition, HWI | Min 120 sec | Min 120 sec | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80 mm/min | 1 - 3.15 in/min | (+/- 0.125 inch); PLC Code 2; UL 746A |
Thermal Properties |
|
| CTE, linear 68°F | 27 µm/m-°C | 15 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear 68°F, Transverse to Flow | 79.2 µm/m-°C | 44 µin/in-°F | from -40F to 100F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 23.4 µm/m-°C | 13 µin/in-°F | Flow, 140F to 280F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 160 µm/m-°C | 89 µin/in-°F | Cross Flow, 140F to 280F; ASTM E 831 |
| Deflection Temperature at 1.8 MPa (264 psi) | 216 °C | 420 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 140 °C | 284 °F | UL 746B |
| UL RTI, Mechanical with Impact | 140 °C | 284 °F | UL 746B |
| UL RTI, Mechanical without Impact | 140 °C | 284 °F | UL 746B |
| Flammability, UL94 | HB | HB | 0.03 in. |
Descriptive Properties | |
| UL File Number, USA | E121562 | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |