SABIC Innovative Plastics VALOX K4530 PBT (North America)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.41 g/cc0.0509 lb/in³ ASTM D 792
Linear Mold Shrinkage0.007 - 0.009 cm/cm0.007 - 0.009 in/in Flow, 0.125 inch; ASTM D 955
Linear Mold Shrinkage, Transverse0.01 - 0.012 cm/cm0.01 - 0.012 in/in 0.125 inch; ASTM D 955

Mechanical Properties
Tensile Strength @ Break103 MPa15000 psi Type I, 0.2 in/min; ASTM D 638
Tensile Strength @ Yield103 MPa15000 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break4 %4 % Type I, 0.2 in/min; ASTM D 638
Elongation at Yield4 %4 % Type I, 0.2 in/min; ASTM D 638
Tensile Modulus3.56 GPa516 ksi 0.2 in/min; ASTM D 638
Flexural Modulus4.64 GPa673 ksi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength151 MPa21900 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched4 J/cm7.5 ft-lb/in 73F; ASTM D 4812
Izod Impact, Notched0.587 J/cm1.1 ft-lb/in 73F; ASTM D 256

Thermal Properties
Deflection Temperature at 0.46 MPa (66 psi)218 °C425 °F 0.125 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)194 °C381 °F 0.125 inch, unannealed; ASTM D 648

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.