MatWeb, The Online Materials Database
SABIC Innovative Plastics VALOX K4560 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
Physical Properties | Metric | English | Comments |
|
Density | 1.5 g/cc | 0.0542 lb/in³ | ASTM D 792 |
Linear Mold Shrinkage | 0.006 - 0.008 cm/cm | 0.006 - 0.008 in/in | Flow, 0.125 inch; ASTM D 955 |
Linear Mold Shrinkage, Transverse | 0.01 - 0.012 cm/cm | 0.01 - 0.012 in/in | 0.125 inch; ASTM D 955 |
Mechanical Properties |
|
Tensile Strength @ Break | 106 MPa | 15400 psi | Type I, 0.2 in/min; ASTM D 638 |
Tensile Strength @ Yield | 106 MPa | 15400 psi | Type I, 0.2 in/min; ASTM D 638 |
Elongation at Break | 4 % | 4 % | Type I, 0.2 in/min; ASTM D 638 |
Elongation at Yield | 4 % | 4 % | Type I, 0.2 in/min; ASTM D 638 |
Tensile Modulus | 4.48 GPa | 650 ksi | 0.2 in/min; ASTM D 638 |
Flexural Modulus | 6.21 GPa | 900 ksi | 0.05 in/min, 2" span; ASTM D 790 |
Flexural Strength | 174 MPa | 25200 psi | 0.05 in/min, 2" span; ASTM D 790 |
Izod Impact, Unnotched | 8.17 J/cm | 15.3 ft-lb/in | 73F; ASTM D 4812 |
Izod Impact, Notched | 0.961 J/cm | 1.8 ft-lb/in | 73F; ASTM D 256 |
Thermal Properties |
|
Deflection Temperature at 0.46 MPa (66 psi) | 220 °C | 428 °F | 0.125 inch, unannealed; ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 200 °C | 392 °F | 0.125 inch, unannealed; ASTM D 648 |
|
|
|
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
|