SABIC Innovative Plastics VALOX VCF2020 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.41 g/cc | ASTM D 792 |
| Linear Mold Shrinkage | 0.005 - 0.009 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.007 - 0.011 cm/cm | 0.125 inch; ASTM D 955 |
| Melt Flow | 47 g/10 min | 266C/5.0 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 22100 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 22100 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 1.6 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 1.6 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 2.43e+006 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 1.871e+006 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 31800 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 7.2 ft-lb/in | 73F; ASTM D 4812 |
| Gardner Impact @ 23°C | 30 in-lb | Instrumented Impact Total Energy, 73°F; ASTM D 3763 |
| Izod Impact, Notched | 0.6 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | 1 ohm-cm | IEC 60093 |
Thermal Properties |
|
| CTE, linear 68°F | 11 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear 68°F, Transverse to Flow | 78 µin/in-°F | from -40F to 100F; ASTM E 831 |
| Deflection Temperature at 0.46 MPa (66 psi) | 407 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 474 °F | 0.125 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 478 °F | Rate B; ASTM D 1525 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |