SABIC Innovative Plastics VALOX 325M PBT (North America)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.

Physical PropertiesOriginal ValueComments
Density1.31 g/cc ASTM D 792
Water Absorption0.1 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation0.34 % Equilibrium, 73F; ASTM D 570
Linear Mold Shrinkage0.009 - 0.016 cm/cm Flow, 30-90 mil; ASTM D 955
Linear Mold Shrinkage0.015 - 0.023 cm/cm Flow, 90-180 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.01 - 0.017 cm/cm 30-90 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.016 - 0.024 cm/cm 90-180 mil; ASTM D 955

Mechanical Properties
Hardness, Rockwell R119 ASTM D 785
Tensile Strength @ Yield7000 psi Type I, 2.0 in/min; ASTM D 638
Elongation at Break180 % Type I, 2.0 in/min; ASTM D 638
Flexural Modulus340000 psi 0.05 in/min, 2" span; ASTM D 790
Flexural Yield Strength11800 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched30 ft-lb/in 73F; ASTM D 4812
Gardner Impact30 ft-lb Modified Gardner, 73F; ASTM D 3029
Izod Impact, Notched1 ft-lb/in 73F; ASTM D 256

Electrical Properties
Volume ResistivityMin 2.2e+016 ohm-cm ASTM D 257
Dielectric Constant3.13 1 MHz; ASTM D 150
Dielectric Constant3.17 100 Hz; ASTM D 150
Dielectric Strength454 V/mil in air, 125 mils; ASTM D 149
Dissipation Factor0.0014 100 Hz; ASTM D 150
Dissipation Factor0.0098 1 MHz; ASTM D 150
Arc Resistance180 - 240 sec Tungsten (+/- 0.125 inch); PLC Code 4; ASTM D 495
Comparative Tracking IndexMin 600 V (+/- 0.125 inch); PLC Code 0; UL 746A
Hot Wire Ignition, HWI15 - 30 sec (+/- 0.125 inch); PLC Code 3; UL 746A
High Amp Arc Ignition, HAIMin 120 arcs Surface (+/- 0.125 inch); PLC Code 0; UL 746A
High Voltage Arc-Tracking Rate, HVTR10 - 25.4 mm/min (+/- 0.125 inch); PLC Code 1; UL 746A

Thermal Properties
Deflection Temperature at 0.46 MPa (66 psi)302 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)131 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical120 °C UL 746B
UL RTI, Mechanical with Impact120 °C UL 746B
UL RTI, Mechanical without Impact140 °C UL 746B
Flammability, UL94HB 0.033 in.

Descriptive Properties
CSA File No.LS88480 
UL File Number, USAE121562 
UV-light, water exposure/immersionF1 UL746C

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.