SABIC Innovative Plastics VALOX 325ML PBT (North America)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.36 g/cc0.0491 lb/in³ ASTM D 792

Mechanical Properties
Tensile Strength @ Yield55.2 MPa8000 psi Type I, 2.0 in/min; ASTM D 638
Elongation at Break16 %16 % Type I, 2.0 in/min; ASTM D 638
Flexural Modulus2.28 GPa330 ksi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength93.1 MPa13500 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched15.5 J/cm29 ft-lb/in 73F; ASTM D 4812
Izod Impact, Notched0.374 J/cm0.7 ft-lb/in 73F; ASTM D 256

Electrical Properties
Arc Resistance120 - 180 sec120 - 180 sec Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495
Comparative Tracking IndexMin 600 VMin 600 V (+/- 0.125 inch); PLC Code 0; UL 746A
Hot Wire Ignition, HWI15 - 30 sec15 - 30 sec (+/- 0.125 inch); PLC Code 3; UL 746A
High Amp Arc Ignition, HAIMin 120 arcsMin 120 arcs Surface (+/- 0.125 inch); PLC Code 0; UL 746A
High Voltage Arc-Tracking Rate, HVTR0 - 10 mm/min0 - 0.394 in/min (+/- 0.125 inch); PLC Code 0; UL 746A

Thermal Properties
Deflection Temperature at 0.46 MPa (66 psi)179 °C355 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)79.4 °C175 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical120 °C248 °F UL 746B
UL RTI, Mechanical with Impact120 °C248 °F UL 746B
UL RTI, Mechanical without Impact140 °C284 °F UL 746B
Flammability, UL94HBHB 0.03 in.

Descriptive Properties
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.