| Physical Properties | Metric | English | Comments |
|
| Density | 1.22 g/cc | 0.0441 lb/in³ | ASTM D 792 |
| Water Absorption | 0.1 % | 0.1 % | 24 hours @ 73F; ASTM D 570 |
| Viscosity | 1.25e+006 cP | 1.25e+006 cP | Melt Viscosity; GE Test |
| Linear Mold Shrinkage | 0.024 - 0.027 cm/cm | 0.024 - 0.027 in/in | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.024 - 0.027 cm/cm | 0.024 - 0.027 in/in | 0.125 inch; ASTM D 955 |
| Melt Flow | 12.7 g/10 min | 12.7 g/10 min | 250C/5.0 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 39.3 MPa | 5700 psi | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Yield | 3.9 % | 3.9 % | Type I, 2.0 in/min; ASTM D 638 |
| Flexural Modulus | 1.79 GPa | 260 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Yield Strength | 56.5 MPa | 8200 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 32 J/cm | 60 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched, Low Temp | 8.01 J/cm | 15 ft-lb/in | at -22F; ASTM D 256 |
| Izod Impact, Notched, Low Temp | 32 J/cm | 60 ft-lb/in | at -22F; ASTM D 4812 |
| Izod Impact, Notched | 8.7 J/cm | 16.3 ft-lb/in | 73F; ASTM D 256 |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 98.9 °C | 210 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 47.2 °C | 117 °F | 0.250 inch, unannealed; ASTM D 648 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |